Solar kiln drying queries

7/14/15       
Peter Bouchard Member

We are designing and building a solar kiln for use in the tropics at 6o north. The average annual relative humidity is 72.5% and average monthly relative humidity ranges from 69% in September to 77% in June. Over the course of a year, the temperature typically varies from 22°C to 32°C and is rarely below 21°C or above 34°C.

We are planning units to comfortably hold 6000 board feet. These will be powered with three DC solar-powered fans for circulation and regulated with vents for internal/external air flow options.

A few questions:

The walls are planned to be concrete block as this is a better insulator than wood – any problem with this?

The roof slope will be around 5 degrees as the sun passes directly overhead during the year, so just for water run-off. This gives us a kiln of around 15 feet in height all round. We were planning to put the fans low down on the input side of the inner wall to suck the air over the heat absorber plate and then down to the fans. But we need to get the air to the upper part of the stack as well, so maybe siting the fans part-way up the inner wall is a better idea – maybe 4 of 5 feet from the ground. Any ideas on this?

Are baffles on the absorber a good idea – will they increase the air temperature by much?

What would be the best recommendation for MC, RH and temperature probes for remote reading in the office close by? These would also read the outside temperature and RH.

Appreciate any answers and experiences – thanks.

9/8/15       #2: Solar kiln drying queries ...
GeneWengert-WoodDoc

I have made several solar kilns for the equatorial tropics. I used the Virginia Tech design.

Regarding the absorber, you do not get any benefit from using an absorber plate versus just painting the interior flat black. You do not have any benefit from baffles on the absorber. The reason is that you are limited by the solar coming in through the clear roof and not the absorber.

For 6000 BF, you need 600 sq ft of roof.

The roof needs to be two clear layers; separation distance is not critical.

We want an insulated wall that also does not store much heat. If it is not well insulated, we lose the solar heat. If it absorbs heat, then the maximum temperature in the kiln and its low humidity is lost. For both reasons, we do not use masonry walls, unless you also put adequate insulation on the inside.

I have not seen moisture probes used with a solar kiln. They would not be useful as their accuracy is probably not good enough. Temperature and RH sensors would be fine if they can withstand frequent exposure to 100% RH...many cannot. But, why do you need such instrumentation? Will you change your operating procedures?

You are correct about the lower fans being poor. However, to comment about the location, we also need to know species, incoming MC, sticker thickness, pile width, vent locations, and fan volume. For simplicity, the standard location on the top near the rear wall seems easiest with vents on the rear wall.

9/8/15       #3: Solar kiln drying queries ...
Peter Bouchard


Hello and really many thanks for your time and feedback.

I appreciate your comments and have – since I posted – done some research on design, and especially the Virginia model. I’m now looking at a 2000 BF unit, which will be 200 ft2 roof area. Because we are 6N, the roof must be almost flat, which means that the ground area is pretty large – 30 x 20 feet for 6000 BF, but the wood itself of course occupies a lot less than that inside the kiln.

I am working with a stack width of 6 feet and a stick height of ¾ inch. I take your point on the collector and thanks for that – it saves putting a collector there at all. I can get black plastic sheeting which will form a separation.

I now plan to fit the fans high, near and inside the intake, so they push the air through the system rather than suck it.

I’m not sure what you mean by the roof needs to be two clear layers. I was intending to use corrugated clear plastic sheets for the roof. I figured this would allow the energy to penetrate and heat the air inside. Where does the second roof layer come in?

I am looking at the air space volume above the stack in the Virginia model. It seems that this space needs to be quite large to avoid overheating? In other words, can we build a kiln with say a 2-foot air gap above the stack (and fans pushing air through that space) or must we increase that vertical gap to 3 or 4 feet? I am thinking the larger space is better.

I am using 3 fans at 1000 cfm on a 2000 bf stack based on 12-18 foot boards. This works out at a tad above 3000 the cfm required air flow, so seems enough. I’m now using a totally wooden kiln.

Will RH and temperature readings change operating procedures. A very good question. I had imagined that, assuming we got a high RH outside, then we would shut the suction and recirculate. The converse would also be true. What’s your take on this? I know that we need to measure the MC ideally using accurate scales on test pieces to get a real idea of how well we are drying the timber.

To give an idea for calculation purposes, we would say Crabwood (Carapa Guianensis) at 30%MC from the bush. Sticker thickness ¾ inch, stack width 6 feet, exhaust vent locations spread to give maximum spread, fan volume 3000 cfm.

Really appreciate any input you can give and thanks once again for your help

Peter Bouchard

9/8/15       #4: Solar kiln drying queries ...
Gene Wengert-WoodDoc

Glad to hear that some of the comments were very useful.

Two layers will improve kiln efficiency by 50%. The second layer can be under the corrugated and can be flat. If you frame the roof with 2x4, then put the flat on the back side and the corrugated on the top.

Regarding high humidity, if the humidity outside is 100% RH and you bring that air into the kiln, then heating it to about 25 degrees warmer will give you about 30% RH. So, what we want to do is to vent a little bit, when the sun is shinning to exhaust damp air and bring air in cooler moisture air that when it gets heated will be dry, pick up moisture (dry the wood), and then be exhausted as more humid air, etc. So, try and get the kiln 25 degrees F hotter than outside...if it gets hotter, then vent more. Usually, the vets are set once and then stay that way for 24 hours. The fans are not run at night when there is no solar heating.

If you like the smaller kiln, then build a second or third one rather than build a large unit.

With a large slope to the roof, the empty space is automatic. With you kiln, I would make the space on top about 24" in the rear to hold 24" fans and then decrease the slope tot he front by 6 degrees. Blow the fans toward the front.

9/9/15       #5: Solar kiln drying queries ...
Peter Bouchard

Again, many thanks for your time. I’ll take all this into account in our design and operation.

I am assuming you mean the lower layer of plastic would be normal Perspex clear plastic sheeting. This is quite expensive where we are – could we use polythene sheeting as a lower layer? Just an idea.

Agree on the smaller kiln – several 2000 bf kilns will work good.

I’ll keep in touch on here and again many thanks,

Peter Bouchard

9/9/15       #6: Solar kiln drying queries ...
GeneWengert-WoodDoc

You can use inexpensive poly film, but it will get brittle and tear from the fans in maybe six months. So, maybe keep your eyes open for a replacement film.

9/9/15       #7: Solar kiln drying queries ...
Peter Bouchard

Thanks, yes, I'll keep an eye open.

Cheers,

Peter

2/21/22       #8: Solar kiln drying queries ...
Avery Smith Member

I’m not sure what you mean by the roof needs to be two clear layers. I was intending to use corrugated clear plastic sheets for the roof. I figured this would allow the energy to penetrate and heat the air inside.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Forestry.com
      Forestry.com is a specialized platform with educational content and equipment for Loggers and Foresters
    • Baker Products
      Industrial Woodworking Machines, Wooden Pallet Manufacturing Machines, & Portable Sawmills
    • Rose Machinery
      Horizontal Band Re-rips, Standard & Custom Designed Machinery
    • Carter Products
      Band Saw Guides, Blades, Wheels, Tires, Line Lasers and 2D Projectors, Wide Belt Sanding Accessories, Vacuum Holding Systems and More

    Become a Sponsor today!