Subject: Re: high flash Naphtha softens CAB Lacquer

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

high flash Naphtha softens CAB Lacquer

5/4/16       
Jeff-1

I have to re spray a piece that was finished with CAB lacquer and then waxed.
A vinyl sealer was used under the CAB also.

When I used Naphtha to clean off the wax, it started to soften the CAB lacquer topcoat.

It's my understanding that Naphtha should not have the solvent strength to do this and should remove the wax while leaving the CAB unaffected.

The CAB had been sprayed the day before and dried overnight, so it may have been a bit green still, but I wouldn't think that should be an issue.

Any idea what's going on? Or am I just misinformed about Naphtha?

5/4/16       #2: high flash Naphtha softens CAB Lacq ...
Leo G Member

Why was wax applied so soon after the piece was sprayed. Or did I misunderstand something.

5/4/16       #3: high flash Naphtha softens CAB Lacq ...
JeffA

So now you have learned a lesson. If I said it should have worked, then what? It didn't and that's that. You now have knowledge you didn't have before. So, is the lacquer fully cured? What does the technical data sheet say? Probably not, don't you think? Most coatings don't get any testing done on them for at least 2 weeks after finishing. This is the normal time frame to consider full cure. Of course this is a lacquer, which has only the ability to protect the wood from dust. I can't tell what the data sheet says is full cure, you could always call the manufacturer.

5/4/16       #4: high flash Naphtha softens CAB Lacq ...
Robert Member

Hi Flash Naptha is hotter than regular VM&P Naptha. The wax or how soon you applied the wax ( although a bit too soon ) had nothing to do with it lifting the CAB Lacquer, its just a hotter solvent.

5/5/16       #5: high flash Naphtha softens CAB Lacq ...
Jeff-1

The wax was not a paste wax, more of a liquid polish and was not applied until the CAB had dried overnight.

Finish schedule:
1. Dye stain on Maple.
2. Wash coat of Vinyl sealer (50/50 mix)
3. Scuff and wipe stain (SW BAC)
4. Full coat Vinyl sealer @ 4 mills wet.
5. Scuff and 1 coat of CAB Lacquer @ 4 mils wet.
6. Air dry overnight at approx 75 degrees

The application of wax (polish) is standard practice by the shipping and QC people to remove any handling marks, fingerprints etc before packing and shipping.....not my call.

@JeffA, I don't need a scolding, just looking to increase my knowledge of the products when they don't behave they way they are theoretically supposed to.

5/5/16       #6: high flash Naphtha softens CAB Lacq ...
Jeff-1

@ Robert:

That's what I suspected might be the case but even then I wouldn't think that an oily, Aliphatic solvent would have the strength to soften the CAB lacquer.
But apparently the difference between the V&P and High Flash blends is significant enough to make a difference in the way it interacts with CAB.

And for the record, it didn't lift the CAB, it just softened it up to the point where it was beginning to show rag marks and probably would have gotten worse with continued exposure.

5/5/16       #7: high flash Naphtha softens CAB Lacq ...
Robert Member

Good thing you stopped when you did, the softening would escalate to lifting had you continued applying it.
Lacquers formulated for today's application don't have the same twigs and berries they once enjoyed.

5/5/16       #8: high flash Naphtha softens CAB Lacq ...
chris

is the CAB lacquer pre catalysed?
used to spray a lot of it when non catalysed but then chemcraft changed formula to be a precat.
after that i had a lot of problems with it.

5/6/16       #9: high flash Naphtha softens CAB Lacq ...
ThomasFR

No experience with high flash naphtha but having done spot finishing (touch up) for many years it was common to wet sand nitro lacquer with naphtha or mineral spirits. Non issue till using a generic "paint thinner" as used to reduce oil based enamel. Found out quickly that formula had some hotter solvent(s) in it & did "soften the lacquer. After 24 hrs dry/cure could proceed as usual. Hope you can salvage the job without compromising the result.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)