3/19/15       
NH Ken Member

So, I just refinished a top for a client; I originally used Waterlox but they cut through it in three months with rough cleaning and scouring pads.
I am somewhat new to table tops, but I did my research and chose Behlen Rockhard Tabletop Varnish; the new kind with Poly.
Per instructions from woodworking videos, I brushed on a few coat, tipped it off and it did NOT flow down the next day.....major brushmarks as well as a few craters. Clearly, I am doing something wrong (I think). So, I thin the next coat down 25% and it flows pretty well. Same with the next. However, my previous "sins" were extremely hard to erase. I ended up trying to wipe on some coats with thinned varnish; it flashed to hardness almost immediately, leaving rag marks.
I let it cure, then sanded 400, then 600, then 800, Steel Wool, then merzernas polishes. It took forever. I can still see my scratch pattern, but have been told this is what it should look like if you hand finish your projects. Overall, I give myself a B.
So, question, is this always going to be this difficult? I must have at least 8 hours into sanding/polishing this single table top...had not counted that into the final cost. Is there an easier way to build up polyurethane top coats? Laying down three layers then cutting through them seems less than ideal, but I am new to this. Any thoughts other than sending it out?
Finally, how toxic is this stuff? I have been sanding and buffing for hours, and have white powder (poly dust) everywhere....I have to wonder what I am ingesting, here?
Best, Ken

3/19/15       #2: Rockhard Varnish Question/Rant ...
Robert Member

Check out the MSDS.

3/19/15       #3: Rockhard Varnish Question/Rant ...
tiptop

The first and most obvious question is why did you not spray it in the first place?

3/19/15       #4: Rockhard Varnish Question/Rant ...
Rick Mosher  Member

Website: profinisher.blogspot.com/

There are very few profession shops using Behlens Rock Hard varnish on tables for just the reasons you mentioned. You can apply a nice finish by hand. I would do it by rolling it on with a foam roller and then tipping it off with either a foam brush or a quality china bristle or badger brush.
However I wouldn't EVER finish a high gloss table that way. It just takes too long. I would use polyester to fill the grain and topcoat with a 2k urethane. Like in the link.

Part one of a 3 part blog post

3/20/15       #5: Rockhard Varnish Question/Rant ...
Leo G

There isn't a finish that is going to stand up to rough cleaning with a scouring pad.

3/20/15       #6: Rockhard Varnish Question/Rant ...
John Member

What Leo said. If your customer continuous using scouring pads on it you'll be getting another call in a few more months. Educate your customer about correct cleaning procedures.

John

3/20/15       #7: Rockhard Varnish Question/Rant ...
rich c.

Any good finish does not come easily. Even spray finish needs work. Temperatures, humidity, age of the can of finish, type and quality of thinner, etc..... all factor into every job. Finishing has a LONG learning curve.

3/21/15       #8: Rockhard Varnish Question/Rant ...
Jim

Pretty well convinced I won't live long enough...........

3/21/15       #9: Rockhard Varnish Question/Rant ...
NH Ken Member

Thanks for the feedback, guys. Glad to hear I am working with a difficult product...if I ever need a shiny awesome tabletop, I will send it your way, Rick.
So I am not crazy in getting a little flustered about the scouring pad? I feel much better, thanks.
Ken

3/21/15       #10: Rockhard Varnish Question/Rant ...
Leo G

Ask them if they would use a scouring pad on their hutch.

It's finished so it will be easy to clean. At worse you put a damp cloth on the dirt and let it sit for a minute or so to soften the smutz and then wipe it off gently. If you are scrubbing the finish off in 3 months then you are doing all kinds of wrong to that top.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)