Need Tips For orange Peel

8/11/15       
Rob Member

Hi Guys I am a little green behind the ears and I am still learning.

I just completed a kitchen reface for my in laws that came out ok, but I am having issues of getting a little orange peel with my spraying.

I want that real smooth Glass like finish and it is bothering me.

I am using a cheap( 45.00) husky siphon feed quart cup gun model h4930ssg.
I am using ML Campbell precat sealer and ML Campbell pre cat lacquer.

I am thinning my material about 15 to 20 percent with lacquer thinner. I live in Phoenix Az where it has been really hot right now and a little humid as well (monsoon).

I am putting on 2 coats of sealer (sand after each coat) and 2 coats of Lacquer.

My Husky gun seems to not atomize as well as I would like it to, I dont know know if its because of my gun or maybe not thinning enough, or too many coats.

I have a harbour freight hvlp and I dont use it because it leaves a lot of orange peel as well.

I want to buy a new gun but I am afraid to get an hvlp if it leaves orange peel, I have a small shop and I am eager to learn, any advice I would sure appreciate thanks.

8/11/15       #2: Need Tips For orange Peel ...
JM

HVLP is not the cause of orange peel.

There is a direct correlation between temperature, gun needle/tip size, and amount of thinner required.

Then there is technique, too much and you get orange peel, too little and you get dry spray.

Then there is gun setup, are you using enough atomizing air?

For your sealer and lacquer, a tip in the area of 1.4 to 1.8mm will work fine, and you probably want somewhere around 20psi at the gun with the trigger pulled. Dont read the pressure gauge at the tank, there are losses in the line. Get a little restrictor with a gauge and put it right at the gun to dial your air pressure in.

Get a wet film thickness gauge. Spray coats in the 3 to 5 mil range.

Hold gun about 6 to 8 inches from the part and make 50% overlap with each pass.

Above information should be enough to get you started.

8/11/15       #3: Need Tips For orange Peel ...
JP Member

Since you want to learn that is the first and most important step. The above is very good advice. You learn that and just about any equipment will work. With that said, if your up to investing in a new gun, you might want to consider CA Technologies CPR gun with a 3M PPS cup.

I say this because you said you are spraying ML Campbell. CA Tech's site has all the info you need for using ML Campbell products and their equipment (Tip sizes, Viscosity, etc). Plus the CPR guns come as both compliant and HVLP. The best of two worlds. And they are just a phone call away. Their customer support is great.

When I first started spraying, my supplier was a distributor for both. I trusted them and all went well. I now use the CA Tech AAA pump. I need the volume it provides.

So learn to get the viscosity straight for your conditions and deal with the tip you need for your gun. They seem to go hand and hand.

8/11/15       #4: Need Tips For orange Peel ...
Robert Member

Once in awhile, adding a bit of Retarder to your mix will help. It slows down the dry time and allows the coating to flow out. Experiment on some sample pieces and see how it works out.

8/11/15       #5: Need Tips For orange Peel ...
afinisher

Using more reducer is worth a try. I wouldn't hesitate to go to 40 or 50%. Use the manufacturer's reducer- the slowest one they carry for your geography. I would try to get ML tech support to help you get to what you need. Off the shelf lacquer thinner won't cut it.

Precats are high solids and standard lac thinners are fast and loaded with acetone which the govt loves for low voc. However- acetone is difficult to slow down the flash of your coating. Fine in Minnesota but impossible in Phoenix.. Hence, more reducer will help flow out but I still prefer a reducer without large % of acetone but that is getting very hard to find these days.

I would talk to Campbell support- Reducer is important.

8/11/15       #6: Need Tips For orange Peel ...
rich c.

Cheap guns, cheap finish. Go to an automotive paint supplier and get a gun. Stop shopping where they only sell Chinese knock-offs. By the way, a lot better finishes than lacquer for kitchens. It's going to fail around the dishwasher, sink, and stove in just a couple of years.

8/12/15       #7: Need Tips For orange Peel ...
Mastercabman

What kind of compressor are you using?
Does it put out enough CFM?
Most of those cheap guns are old technology and uses a lot of air
If your compressor don't put out,your material is not going to atomize properly
Today there are HVLP guns that uses low CFM and you can use a 2hp small compressor
As for thinning I use a flow enhancer
C163 for MLC product
10-20% should do it

8/13/15       #8: Need Tips For orange Peel ...
Rob Member

Hey thanks a lot for all the help I have received from everyone.

I did some of the suggestions I have gotten and I was able to get a better finish.

I think I need to get some retarder because it is hot down here and I am getting a little dry spray, I have to make a pass about 4 time before it becomes a wet coat.

I am going to get a good gun I just dont have the money yet, i also dont know what to get...AAA or hvlp any suggestions ?

I really dont know the benifits between the two different types.
Again thanks for any advice it means a lot to me.

8/13/15       #9: Need Tips For orange Peel ...
Robert Member

Greetings Rob, what sort of compressor are you using /tank size/ horse power. Do you have a separate oil/water filter?

AAA is air assisted airless, totally different animal.

Devilbiss has a decent set of HVLP guns with various nozzles/tips/caps.
With the same gun you just change out parts and pieces to adapt to the various coatings. Primer/sealers/coatings can all be sprayed out of the same gun.
Amazon has some decent deals on them and for the money they lay out a nice finish.

8/13/15       #10: Need Tips For orange Peel ...
Robert Member

Whoops....didn't see Mastercabmans posting where he asked some of the same ?'s I just did. Sorry for stepping on your toes.

8/13/15       #11: Need Tips For orange Peel ...
Mastercabman

Robert
No problems!
I think we need to know what the OP has as equipment before we suggest what he should need

8/14/15       #12: Need Tips For orange Peel ...
Rob Member

Hey guys I have a 80 gallon Kobalt air compressor that runs off of 220 I don't know the amount of horsepower I can check when I get to my shop.

I just put a regulator that has a water release on it but I don't know if its the same as a oil water trap.

Robert the develbiss hvlp spray guns sounds cool but I'm a little leary on hvlp because of the heavy orange peel i was getting, but i am sure it was because harbor freight.

Do u think it will atomize it well enough with out over thinning to be able to give me a good finish

8/14/15       #13: Need Tips For orange Peel ...
Shane

I work in a shop that finishes over 20 million dollars worth of custom architectural millwork a year. we have finish equipment that ranges in the hundreds od thousands of dollars... we have very expensive spray guns around here and cheap crappy harbor freight ones laying around for little dirty jobbers. I can spray out a panel with the HF gun with the same material that's sprayed in a $600 Sata and get the same results. it's all about tailoring your coating to your equipment and environmental conditions. Yes I may have to use a little more or less air pressure to get it to atomize.... yes I may add some percentages of Butyl Cellosolve to the mixture of a pre-cat or conversion varnish. It comes down to proper technique ( I.E. part distance, overlapping, wet mill thickness )adjustments to your coating..... I've shown my guys here it can be done.... same thing as "Chrome won't get you home"....

8/14/15       #14: Need Tips For orange Peel ...
Robert Member

I have a hunch Rob that the orange peel is due to user error and partially the fault of your equipment ( yer spray gun ). Not going to slam the HF/Husky spray gun but other brands of guns offer different needles and caps and nozzles that are matched to the material your applying.

An 80 gallon tank is large enough to facilitate the use of just about every spray gun on the market. The main advantage to the HVLP is there is very little over spray; you will realize good transfer efficiency using them or the LVLP.

Not pushing DeVillbis but they are a good step up from the Harbor Freight/ Husky and wont break the Bank. They also make a reasonably priced oil/water separation unit.Both water and oil can wreck havoc on a coating.

If you have time, check out some YouTube videos of HVLP demonstrations. You can get a glass smooth finish, but like everything else, its gonna take the patience to practice and the willingness to experiment.

8/14/15       #15: Need Tips For orange Peel ...
Adam

Buy an Astro HVLP gun from Spraygunworld.com. They are definitely capable of Sata quality finishes and they cost under $100. The 80 gallon is probably 5HP and has plenty of guts. The Astro HVLP are actually high transfer guns that are 65%, but atomize at a better rate than the higher efficiency hvlp guns.

You could buy a cheap gun from Harbor freight and that weeks batch might be okay, but the next weeks are all junk. No quality control.

8/15/15       #16: Need Tips For orange Peel ...
Rob Member

Thanks guy for the responses Robert thanks for the PM.

I think you guys are right and that a lot of the orange peel is from me not shooting correctly, or tuning the fluid, fan, air flow correctly, retarder etc.

With that being said,
I dont mind spending up to about $2000.00 on a good gun. I will wait till my next big job and then will buy something better. The husky was referred by a friend that why I bought it and the harbor frieght was a cheap turbine that I could bring to the job with me.

I really dont mind spending some money on a good gun/guns. But I am confused on what to get because there are different types of systems pressure pots, hvlp, lvlp, Airless, Air Assisted Airless. Siphon feed. etc.

I once seen a guy with a AAA and thought wow what a cool gun but for a rookie and a small shop should I buy one or start with a nice hvlp, and should the hvlp be for spraying cars or woodworking? is there a difference?

Or should I go in the middle of the road with a pressure pot, but then I still have to buy a separate gun (I think)

8/15/15       #17: Need Tips For orange Peel ...
Robert Member

You can either purchase something for the present or purchase something for the future. Thats a call for you to decide.

An all in one website that pretty much explains in basic "talk" the answers to your questions is....CA Technologies.

That should keep ya busy fer awhile.

8/15/15       #18: Need Tips For orange Peel ...
rich c.

A major concern for new equipment is how often and how many different finishes will you be using. Also will you graduate to catalyzed finishes. Get an airless, or pressure pot, and you get to clean hoses plus the gun. And then with a deadline if you use catalyzed. Flushing hoses is a big deal. Get a good gun with gravity cup, and all you have to do is clean the gun and cup. I much prefer gravity cup vs suction cup.

8/16/15       #19: Need Tips For orange Peel ...
scott

I know that everyone has different needs and expectations but I have used most everything over the years and the AAA systems are the best for spraying, the new ones you can turn the air pressure down and get very little over spray. I will admit they have to be cleaned and they need to be used fairly often so seals stay conditioned, but they are the best. If you are only doing a few pieces and only need to mix small amounts of material I use a Sata gravity feed. For woodworking you only need the 100 model with about a 1.8 tip and they spray great, the sata guns use the disposable cup system also which is awesome.
All the best.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)