Finishing schedule:

1. Walnut lacquer stain sprayed on, light wipe.
2. Let stain dry 45min. or longer.
3. Spray full wet coat of nitro lacquer sanding sealer.
4. Let dry overnight and sand with 220.
5. Spray on BIN shellac base primer tinted
to desired color.
6. Let dry 1 hour.
7. Sand primer with emphasis on profiles and edges back to stained wood for distressed look.
8. Top coat with full wet coat of Minwax Polycrylic satin.

I made two samples with one having the shellac primer tinted to another color. The first time I did not get this crazing. The first sample I may have let the shellac dry longer before distressing and applying the polycrylic, but not sure on that. Also, I put the sample in front of a shop fan to speed drying of the polycrylic after it tacked up, but did this on the first sample as well, just not sure how long I let it dry before doing that.

I thought this BIN primer could go on just about anything and be topcoated with anything. I use it a lot as a primer on opaque paint jobs, and was using here because it drys fast and sands well.

Any ideas as to why I'm getting this crazing??


View higher quality, full size image (3000 X 4000)

11/22/16       #2: Crazing of polycrylic over shellac ...
rich c.

Ideas? Maybe because you used 6 different kinds and brands of finish on it. Likely something wasn't fully dry before coating again. Just get some conversion varnish tinted and spray one product.

11/22/16       #3: Crazing of polycrylic over shellac ...
Steven

Thanks for replying, but I wouldn't even consider using conversion varnish unless I was building a kitchen or bath cabinets. Nitro lacquer is about as toxic as I'll go with finishes for the mostly built ins and furniture type cabinetry I build that wouldn't get the type of use that would necessarily warrant a conversion varnish or similar finish.

I wasn't having problems with the shellac on lacquer sanding sealer so I'll take your advice and try another sample and let the primer dry for several hours or so before sanding and topcoating with the polycrylic; or can someone recommend another water clear finish that would be compatible with the BIN primer?

I guess if I had to I would try and get some white nitro lacquer tinted to the color I need and topcoat with a CAB acrylic lacquer, though if I remember from a demo can I got a while back it was pretty nasty smelling stuff too.

11/22/16       #4: Crazing of polycrylic over shellac ...
Leo G

Stick with the nitro. Or start with the polyacrylic. Don't mix so many finishes.

11/22/16       #5: Crazing of polycrylic over shellac ...
Nick

I agree something in there wasn't dry.
what are you spraying the pigmented shellac with? I know you have quite few steps already...but try 2 light, thin coats with at east 45 minutes try time between coats...hope that helps.

11/22/16       #6: Crazing of polycrylic over shellac ...
Denny J

The shellac was not dry. I would suggest switching to all water based products and those issues will disappear. General Finishes has a range of products that all work together that can give you just the look you are trying to achieve.

11/24/16       #7: Crazing of polycrylic over shellac ...
Adam

Why use sanding sealer if you are going over it with primer? If you are hell bent on sanding sealer. Switch to shellac based Sealcoat.

How long are you waiting between the BIN and wb?

11/24/16       #8: Crazing of polycrylic over shellac ...
Michael Foscone

Steven,
Sorry you had problems and some rude replies. The Shellac tinted primer was not fully dry, I suspect it felt dry and even sandable, but not completely dry. When your coat of poly was applied on top of that, it trapped the primer and the crazing was caused because the primer is a considerably slower dryer.
I thank you for bringing the problem up, I am always looking for new finishes, and I shall use this one with a little modification on some antique reproductions.

11/24/16       #9: Crazing of polycrylic over shellac ...
Steven

Thanks all for the additional responses. The reason I'm using a sealer over the stain, before primer, is to create a layer of protection to avoid rubbing into the stain and lightening it or rubbing to bare wood.

You can see in this picture that I also used a heat gun on the corners and in random spots to create some lifiting/bubbling of the primer that could be scraped off for effect. I believe the lacquer sanding sealer did not bubble up with the shellac and that ended being a benefit to protect the stain while I did the rub through.

Yes, SealCoat would have made more sense before the primer as they're both shellac products but is difficult to come by in my area; I'd have to order online to get gallons and drive an hour to a Rockler store just to get expensive quarts. A lot of the products mentioned are not available locally, and I've called around quite a bit over the years looking for a knowledgeable supplier. In my area, it's mostly stains, water and oil paints and clear lacquer and polyurethanes. Good luck trying to find a store that can tint a lacquer or conversion varnish or even carries them in white, and even if I were to have them order me some, they wouldn't have the colorant system to tint them.

I finished another sample after giving the primer more time to dry and it did not craze this time; the label clearly states that the addition of UTC colorants will cause the primer to take longer to dry; I should have heeded that warning.

On another note, this crazing/alligatoring effect might be desirable for this antiqued look in some instances, except that I don't know if I could reliably reproduce it, lol.


View higher quality, full size image (1024 X 768)

11/24/16       #10: Crazing of polycrylic over shellac ...
RobertJ

I cannot add anything to the process, but I do like the finished look even thought it may not be consistent.....it may appeal to your client.

12/5/16       #11: Crazing of polycrylic over shellac ...
Mike Fleck

Website: http://www.fleckelectric.com

I found this post investigating my own issues with lacquer tenting over shellac. Wondering if the BIN was old. My shellac I made was old but it was able to be sanded in minutes so I felt it was usable. Later on another project I noticed that I could still thumbprint shellac weeks after applied.

1/5/17       #12: Crazing of polycrylic over shellac ...
Steven

I wanted to post a follow up to this. I used this finishing process(except I let the shellac primer dry overnight before light sanding, distressing, and topcoating) on a built in that I stored for almost a month in my shop before installing and it was holding up fine and the acrylic/urethane topcoat seemed to be pretty durable. I actually ended up using Kelly Moore's Kel Thane II instead of the polycrylic.

Here's a pic to show the lightly distressed look I was trying to achieve.


View higher quality, full size image (4000 X 3000)

1/5/17       #13: Crazing of polycrylic over shellac ...
Michael Foscone

Very nice Steven, glad it worked out so well.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)