8/4 Cherry Top moisture content?

5/10/18       
Michael Member

What moisture content should I have my lumberyard make 8/4 cherry wood boards at so that I can avoid any warpage?
Size of the top I will be building is 22''x142''using 8/4 cherry. Thank you!

5/10/18       #3: 8/4 Cherry Top moisture content? ...
rich c.

6-8% Narrow boards are better, nothing near the pith and minimal sapwood on both sides. Quarter sawn is even better.

5/11/18       #4: 8/4 Cherry Top moisture content? ...
Mike Member

Rich, would you say 5'' in plain sliced cherry is narrower enough? I like to use quarter sawn but customer wants to see the feathers. Thank you!

5/11/18       #5: 8/4 Cherry Top moisture content? ...
Mark B Member

Do you literally have a supplier that is letting you call our the MC for a given order? That would be wild.

Our suppliers run material to industry standards. There is no asking for a half dozen boards to be taken to any given MC?

If your buying high quality material from a supplier that either saws their own material (and knows what they are doing), or sources from trusted sawyers, your source material should be of no concern.

We buy a good bit of plain sawn cherry from 4/4 on up from a spectacular supplier and have never had an issue. Any issues with regards to the material itself. Any issues will likely come from within the four walls of your shop.

5/11/18       #6: 8/4 Cherry Top moisture content? ...
rich c.

I'd say just under 6" width in this case. That uses 4 boards and then trim to width.

5/12/18       #7: 8/4 Cherry Top moisture content? ...
Mike Member

rich c, thank you!

5/13/18       #8: 8/4 Cherry Top moisture content? ...
Gene Wengert

The old adage of 6 to 8% MC really means 5.5% to 8.5% MC. This range is too much and for an interior table in a home is way too high. In most of the US, you would want 6.8% MC to 7.0% MC to avoid most warp. Note that ‘this is equivalent to 35% RH. Do you know the RH in the home or office, especially in the wintertime? Is it drier?

Note that any change in humidity will change the MC and this will result in size change including warp. A typical home runs from 30% RH to 50% RH (winter to summer) average which is 6.0% to 9.0% MC in the wood. This will result in over 1/3% size change in width, winter to summer. So do not fasten the top firmly to the frame, but allow for movement in width.

Also, make sure both top and bottom are finished the same so you get even moisture changes, top and bottom. This will really help prevent warp.

5/14/18       #9: 8/4 Cherry Top moisture content? ...
Mike Member

Gene Wengert, thank you!
I like the idea finishing underneath of the tabletop.

5/14/18       #10: 8/4 Cherry Top moisture content? ...
Tennessee Tim  Member

Website: http://www.tsmfarms.com

Always finish ALL sides of furniture with at least one good coat I use minimum of 2.....On the first round I always do the back (hidden) side first and immediately flip and do the other, this prevents usual MC changes from overnight drying in shops NOT having controlled MC/RH warping top. ALSO sticker up high for better airflow in drying. This makes MC changes equal on the wood and keeps good balance. ALSO correct joinery prevents future failures....tops need to float (actually any crossgrain woods)...NEVER glue wood cross grained.....VERY, VERY few exceptions!!!
Check out my website re wide slabs and furniture.....IT'S ALL about knowing the wood and good joinery!!!

5/16/18       #11: 8/4 Cherry Top moisture content? ...
DaveM Member

Gene, Perhaps I am confused, but I am in the southern tier of Western N.Y. & the humidity in my house in the summer averages between 60 & 70% according to my "weather station". Winter is between 30 & 50%. Maybe RH is a different measurement than what my electronic unit is giving me. I only post this as I have made most of the furniture in our house & all the wood was air dried / shop dried to between 10 & 11.5% & I have not experienced any warping or stress cracks. Although, as has been suggested in this thread, all tops have been attached using figure 8 fasteners, not glued.

5/17/18       #12: 8/4 Cherry Top moisture content? ...
Mike Member

Tennessee Tim, thank you!

5/17/18       #13: 8/4 Cherry Top moisture content? ...
Gene Wengert

The outside RH in western N.Y. averages 70% RH in the summertime. It is below this during the day and higher in the nighttime, especially before sunrise when dew forms on the grass, etc. we can have the drier conditions in the daytime inside a house, but the high humidity in earlier morning will not happen in the house, as it is a bit warmer in the house and such high RH would be uncomfortable. It is therefore very unlikely that the inside of a home will be equal or more humid than the outside. Further, when humid outside air is heated such as in the winter, the RH quickly drops. Foggy air drops to under 30% RH with just 25 degrees of heat. So, the bottom line is that I suspect the weather station you have is not very accurate...your readings do not agree with the readings that others have taken.

Air dried followed by drying in the shop can achieve reasonable low moisture contents, even though the wood was not "kiln dried."


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)