Subject: Re: Veneer curling

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Veneer curling

9/12/13       
Dan Member

Just started Veneering our substrate with Hardwood veneers and we are having troubles keeping the 9" wide by 80" long maple veneer from Curling up before pressing. As soon as we place the veneer on the glued substrate we start to see them curl up like a canoe.

Any ideas on why this is happening. Veneer to dry and as soon as we put it on the glue its taking in moisture?

Thanks ahead for any info.


View higher quality, full size image (1296 X 968)

9/13/13       #2: Veneer curling ...
Chaim Gottesman

You are using a water based glue so as the veneer takes on moister it cures like a potato chip!
try a different glue that isn't water based!
Chaim

9/13/13       #3: Veneer curling ...
Charles  Member

Website: http://www.northcreekwoodworks.com

Random thoughts:
Your veneer (or plant) MC may be low. We do not get this very often as our veneer is 7-8%.

Place the veneer on the core just before you put it into the press, no lingering. You could even place the top veneer on in the the press as ir seems you have a manual feed press.

Make sure there is no direct hear flowing on the layup table. (a winter issue).

FYI (not related) I have 125" guillotine F/S in the Machinery exchange; if you can use one it's good deal. Really need it out of here.

9/13/13       #4: Veneer curling ...
rich

Are you applying a coat of adhesive to the veneer? Or just substrate?

9/14/13       #5: Veneer curling ...
Rich

Simple solution been doing this for years. Take a clean spray bottle, fill it with clean water, distilled water if you feel more comfortable, doesn't matter. Hold the spray bottle about 2 feet above the veneer and with a sweeping motion, lightly mist the veneer. Doesn't take alot just mist it. The veneer will start to lay down before your eyes, it works trust me. What you're doing is basically counter balancing the moisture the veneer takes on from the glue. Works with all raw veneer. Learned this trick back in '89 from a man that was considered at the time, and was, one of the smartest veneer guys in the entire world.

9/14/13       #6: Veneer curling ...
Rich

One additional note, I would cross band and re-calibrate those hardwood edged boards, you're going to have a telegraph issue if you don't. Okume works well.

9/15/13       #7: Veneer curling ...
Dave

With PVA, I only do what can I spread and get into the press within 10min or so. I spread the glue, lay the veneer and lay the cover sheet(s) - a single process with three steps. I use a few short bits of tape, pre-applied to the veneer and cover sheet(s), to keep things from sliding around (better perimeter bond). Curl is unavoidable, but easily handled with tape, cover sheets or stacking (I prefer not to do the later). I would never introduce extra moisture by spraying the face of the veneer w/ water.

What kind of glue are you using, it looks like water based contact cement (not a good choice)?

I agree, unless you need it that big for an edge profile, the banding is way too big.

9/15/13       #8: Veneer curling ...
Rich

I guess if you have the time to go through all those steps as Dave does it, give it a try. A very light mist of water does the trick, it's quick it works and doesn't hurt a thing.Pressed thousands of sheets this way. But everyone has their own technique, find what works for you and run with it. Good luck with your project

9/16/13       #9: Veneer curling ...
Dan Member

Thanks Guys for all the info, ill try a few things and get back to you with what works for me. I am applying glue to the substrate and not the veneer. I also need this wide banding for profiling.

9/20/13       #10: Veneer curling ...
Bob

Based on the picture you are taking too long to get them in the press. You've got 4 double sided panels glued and nothing is in the press yet.

Also no cauls to hold the veneer flat. My veneer curls if I lay in on a fresh glued surface and don't do anything to hold it down, even 1/4" mdf will do the job.

Doesn't seem like a veneer problem but more of a process problem, change the process and the problem will go away.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)