Today's
Sponsors:


Finish Systems

Firth Maple Products

FORDAQ

FormWood Industries

Freeborn Tool Company

Fuhr International

Fuji Spray

Gabbiani Machine

Gary M. Katz

Global Hardwood Flooring

Glue Machinery Corporation

Goby Walnut Products

Graco, Inc.

Granite Road

Grayson Ferguson Woodworking Inc.

Great Lakes Kiln Drying Association

GreCon

GUHDO

Hanson and Leja Lumber Company

Hardwood Council

Hardwood Store of N.C. Inc.

Heartwoods, LLC

Her-Saf

Hermance Machine Company

High Point Grinding - Total Saw Solutions

Historical Plus Wood

CNCROUTERSTORE.com

CNT Motion Systems

Colonial Saw

Construction Programs and Results

Cook's Saw Mfg.

COOLwoodworkingstuff.com

Country Saw & Knife, Inc.

Courmatt International Inc.

CP Adhesives

CSH Custom Service Hardware Inc.

CTS Manufacturing Inc.

CustomMade.com

Cutlist Plus

D.S. Brown Machinery

Dancer Lumber

Delle Vedove USA, Inc.

Delmac Machinery Group

Delta

Denray Machine

DeVilbiss

Dispoz-A-Blade

Diversi-Tech

DMC

DODDS

Don Hall & Associates

Donald Dean and Sons

Durable Wood Products

E.W. Tooling Inc.

Eagle Machinery and Repair Co.

ECabinet Systems

Edge-It Edgebanding

Edwards Wood Products

Electrophysics

Elias Woodwork & Manufacturing

Elkom North America

Emerald Hardwood Floors

Endeavor Hardwoods

EnRoute WOOD

ETemplate Digital Measuring

ETK International

EX-FACTORY

Excel Dowel and Wood Products Inc.

Extrema Machinery

ez-Router

FastCap




20 Steps to Drying Hard White Maple       The Wood Doctor's 100 percent guaranteed, sure-fire, no-snake-oil method for successfully drying hard white maple. 1998.

by Dr. Eugene Wengert

Professor and Extension Specialist in Wood Processing
Department of Forest Ecology and Management
University of Wisconsin-Madison

To successfully prevent enzymatic oxidation staining, it is necessary to dry lumber quite rapidly and to avoid high temperatures, especially above 40% MC. In the case of sticker stain, this prescription means drying the wood under the sticker as rapidly as possible. Certainly, when possible, the logs should be freshly harvested, especially during warm weather. When this cannot be done, then the following procedures should be followed. In some cases, the different measures suggested below may be excessive, but one cannot judge in advance the risk of stain formation. Therefore, doing a little extra should be viewed as insurance. The risk is staining the lumber, which can result in 1000's of dollars in lost income.

Logs
1. In warm weather, always use freshly harvested logs.
2. End coat the logs with a wax-type coating to prevent log end stain.

Stacking & Handling
3. After sawing, in warm weather, stack the lumber within 12 hours.
4. Use stickers between 8% to 10% MC; check the MC with a moisture meter; get the stickers directly from the unstacker rather than from storage.
5. Use stickers no more than 1-1/4 inches wide, by 3/4 or 7/8 inches thick.
6. Use a grooved sticker for a little extra advantage. This sticker allows some air movement under the sticker and thereby encourages the wood under the sticker to dry faster.
7. After stacking, the lumber must be kept out of the rain, especially at high MCs and in warm weather.
8. After stacking, if not loaded directly into the kiln, place the lumber in fast drying locations. Fan-sheds (or blow boxes) would be ideal; air drying is poor.

Predryer & Kiln Equipment and procedures
9. Brush snow off the lumber before entering the dryer.
10. Use a kiln load narrower than 16 feet.
11. Use a velocity over 500 fpm.
12. Do not use a "snow melting" or "thawing" kiln procedure.
13. Develop kiln relative humidities, within the first 6 hours of drying, that are at least equivalent to a 10 F depression. Larger depressions may be required, if recommended in the schedule. In humid weather, kiln temperatures may have to be raised slightly to achieve the low humidities required.
14. Load the kiln with only two rows of lumber rather than 3 or 4 for the first 12 to 36 hours to help achieve the required humidity immediately. Then, after the RH has been maintained for 12 or more hours, load the remaining lumber; the required RH should be more easily achieved in this manner at all times.
15. Use low kiln temperatures (110 or 120 F initially), as recommended in the schedule; never exceed 160 F, except during equalizing and conditioning.
16. Reverse fans every two hours.
17. Use correct kiln sampling procedures.
18. Do not over-condition the lumber.
19. If lumber has been air-dried or possibly mishandled, use a special kiln schedule that operates at very low temperatures.
20. After the first 10% to 20% MC loss, unstack and restack, using dry stickers in new locations.

Professor Gene Wengert is Extension Specialist in Wood Processing at the Department of Forestry, University of Wisconsin-Madison



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Primary Processing: Air Drying Lumber

  • KnowledgeBase: Primary Processing: Kiln Operation

  • KnowledgeBase: Wood Engineering: Wood Properties

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article