Today's
Sponsors:


Vintage Wood Products

VortexTool Co. Inc.

VyTek

W. Moore Profiles, Ltd.

W.L. Fuller

Wagner Electronic Products

WalzCraft Industries

WEIMA America, Inc.

Weinig Group - USA

Western Dovetail

Williams and Hussey

Wisconsin Knife Works

WMIA

WMMA

Wood Doctor's Rx, LLC

Wood Technology Inc

Wood-Mizer

WoodCabinetDoors.Com

WoodenBoat

WoodFinder

WoodJobs.com Search Consultants

WoodLINKS

Woodmaster

WoodPlanet Inc.

WoodSprayGuns.com

WOODWEB

Woodworker's Supply/woodworker.com

Woodworker's Directory

Woodworking in America

Wright Timber

Specialtytools.com

Speed Sander

Spink Lumber

Sprayguncaptain.com

Stefani

Steve H. Wall Lumber Co.

Stiles Machinery

Stiles Shop Solutions

Stoneys Hardwoods

Super Source Tooling Inc.

Supergrit Abrasives

Superior Wood Products

T-Tool USA LLC

Target Coatings

TaylorCraft Cabinet Door Company

Techno CNC Routers

Template Services

The Veneer Store

Thermwood Corporation

Tiger Wood Ltd.

TigerStop

TigerwoodDecking.com

TimberKing

Timesavers Inc.

TMS Machinery Sales

Tomlin Architectural Millwork

Tooling on the Web

Toolstoday.com

Top Drawer

Touch Up Solutions LLC

Tractivity

TradeJobPlacement.com

TradeSoft

Trakware Systems Inc.

TRB Flooring Company

Tropical Hardwoods

True North Cedar

Ubidmachinery Inc.

UC Coatings Corp.

Unique Building Supples

Unique Machine & Tool

University of Wisconsin

UWMO Auctions

VacDry Kilns

Vacuum Pressing Systems, Inc.

Vacuumpods.com

Valspar

Vecoplan LLC

Vector Art 3D

Vectric Ltd.

Veneer Systems Inc.




Abrasive Planing: Gluing and Yield Observations       A comparison of abrasive and traditional knife surfacing of solid lumber, and their effects on gluing and yield. 1998.

by Professor Gene Wengert

Editor's note: The following article is an excerpt from the book "The Wood Doctor's Rx," by Gene Wengert, Professor and Extension Specialist in Wood Processing, Department of Forestry, University of Wisconsin-Madison.

Interest in the abrasive planing of wood has been increasing the past few years, especially with an abrasive planer winning the Challenger Award in 1982 at the Louisville Fair. The abrasive planer is an extremely robust belt sander that uses an abrasive to remove the excess thickness of lumber. Many advantages are possible with the abrasive planer when compared to the knife planer (but not all are important in furniture manufacturing):

- Most machining defects around knots are eliminated (important mostly for knotty styles, as most knots are cut out in traditional styles).
- Belt is changed in minutes rather than knife sharpening in hours.
- Close thickness tolerance is possible (but also true for new knife planers).
- High feed speeds are possible (particularly important for softwood construction lumber).
- Less noise is produced (although newer planers are quieter, too).
- Little change is required for different species.
- Less stock need to be removed to obtain an acceptable surface.

There are a few disadvantages to abrasive planing:
- Belts must be handled and stored with care, usually in controlled RH conditions.
- Power consumption is quite high. (For example, a 24 in. wide abrasive planer may require 250 hp.)
- Dust - a by-product which requires more air and more care in filtering.
- Gluing is slightly more difficult.

We will examine two points concerning abrasive planing that would be of concern to the furniture industry: gluing of abrasive planed lumber, and potential yield benefits of an abrasive planer.

Gluing of Abrasive Planed Lumber
The American Institute of Timber Construction, an industry agency concerned with quality in laminated beams, noted more checking in and near glue joints made with abrasive planed lumber than from knife planed lumber when the joints were exposed to accelerated aging. This was only a preliminary study, so further testing was done. Additionally, in recent months, two furniture companies forwarded samples of glue-line failure problems from abrasive planed lumber to me for analysis (Figure 39-1).

To understand why there could be problems with abrasive planed lumber in gluing, we must analyze the basics. Abrasive planing removes material from wood by scraping. In this process, fibers near the surface, it was discovered by the U.S. Forest Products Laboratory, were crushed and weakened. This phenomenon has been called "sub-surface damage" (Figure 39-2).

In addition to the crushing and distortion of these cells, they also are apparently less tightly attached to the rest of the wood. A comparison of typical surfaces, knife-planed (Figure 39-3)

and abrasive-planed, further illustrates the problems. When abrasive planed surfaces are glued, then, it is analogous to trying to glue the bristles of two paint brushes together end-to-end when the bristles aren't fastened to the handle well.

One characteristic of a broken glue joint will be exceptionally high "wood failure." In fact, in Figure 39-1, the surface is nearly 100% wood failure: the glue did its thing; the wood came apart! Close visual examination of the failed surface, in fact, shows the scratch pattern from the piece above running at a 30 degree angle. The tests by the Forest Service on abrasive planed laminated beams confirmed this observation with wood failure being higher and glue separation being much greater for abrasive planed lumber. Interestingly, the U.S. Forest Service found the best abrasive results wereat 60-grit, not 80- or 36-grit.

What does this mean? Joints from abrasive-planed lumber are weaker than knife-planed due to surface and subsurface damage. This weakness will be further accentuated when the joint is exposed to wetting; the hypothesis is that the crushed cells will swell excessively trying to restore their original shape and that such swelling and resultant stresses will cause failures. Even when there is only slight subsurface damage, the fuzzy surface itself will still cause gluing problems in that it will require more adhesive than normal. (Returning to the paint brush analogy, gluing the bristles together requires more adhesive than just gluing the handles directly.)

However, by increasing the amount of adhesive (spread rate), it is possible (although admittedly we cannot describe when it is and when it is not possible) to obtain a fairly good bond when there is minimal subsurface damage, as the adhesive will penetrate past the fuzz down to "solid" wood.

This would apply to joints not exposed to wetting or exterior exposures. In any case, caution should be exercised in gluing abrasive planed lumber when the joint will be heavily loaded and high strength is required.

Although this is based on abrasive planers, the basic principles apply to abrasive sanders as well.

Abrasive Planing Yield Benefits
The typical abrasive planer for rough lumber uses two heads that are directly opposite each other, one above the other. As the lumber passes between these heads, equal amounts of material are removed from each side--if one head tries to remove more, the forces will push the lumber into the other head thereby providing uniform removal.

Further, the abrasive planer can take light cuts and can, therefore, clean up a board that in an old knife planer might have been rejected. (To be totally honest, new knife planers can also do wonders and, in some situations, a knife planer may cost less than an abrasive planer and may use substantially less power.)

In evaluating new equipment and listening to new users, always remember that they are probably comparing the new machine and results to an ancient piece of equipment. It is true that an abrasive planer, compared to an existing knife planer, has the potential due to a smaller planing allowance to produce thicker planed boards from the same thickness of rough lumber. However, unless this thicker planed lumber can result in improvements in yield in the plant in subsequent processing (that is, unless finished lumber sizes are changed or machines programmed to work more efficiently with thicker lumber) then there is no advantage or benefit. Stated another way, it will take the same amount of rough lumber to produce the same amount of furniture! Of course, if, because of improved planing, the thickness of rough lumber from the sawmill could be reduced a fraction and still provide correct finished lumber thickness (and realistically, I don't believe this is possible at most sawmills), then there could be a saving due to the smaller planing allowance.

Presurfacing
One special potential benefit from the abrasive planer is that by planing lumber green (green = above 50% MC), it will be more uniform in thickness. Uniformly thick lumber will reduce kiln drying time by as much as 25% (Forest Service results on 4/4 oak) and can save 10% of the energy used in a kiln when drying green-from-the-saw. Tests have shown there is no reduction in warp due to uniform thickness, but kiln capacity could be increased up to 11%. (Knife-planed green oak is much less prone to surface checking; this may not be true for abrasive planing due to the tearing effect mentioned earlier.)

Planing Air Dried or Kiln Dried
Air dried lumber that is planed fully (i.e., clean surfaces) will be much easier to defect in the rough mill, as the knots and other defects will be easy to see. An abrasive planer would have an edge over a knife planer in that a clean surface could be obtained on thinner boards more easily.

Lumber planed air dried or kiln dried on new planers will be planed to very close tolerances. This fact now permits reduced machining allowances in subsequent machining (e.g., molder allowance) and suddenly there are tremendous potential yield benefits!

Professor Gene Wengert is Extension Specialist in Wood Processing at the Department of Forestry, University of Wisconsin-Madison



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Adhesives, Gluing and Laminating: Glues and Bonding Agents

  • KnowledgeBase: Solid Wood Machining: General

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article