Avoiding Blush in a Clear Lacquer Finish

      To avoid condensation that causes clear lacquer to take on a milky white blush, keep an eye on ambient temperature and humidity. March 12, 2006

I am having problems with my finish. I am using a nitrocellulose gloss lacquer. It has been raining today and its about 60 degrees in the shop. I keep getting a milky white translucent discoloration with an oil spot quality. I am spraying over about 3 coats of sanding sealer. It appears that a very fine layer of condensation is collecting on all of the recently sprayed finish. Is this the cause of the milky white spots? This has never happened before to me and I have been spraying for years.

Forum Responses
(Finishing Forum)
From Paul Snyder, forum technical advisor:
Going years without ever seeing blush is incredible good luck. To fix the discoloration, you can fog on a very light application of lacquer retarder or spray another coat of lacquer that has some retarder in it. A general rule for spraying lacquer (or shellac) is don't spray if the relative humidity is above 65%. A more accurate guide is don't spray if the dew point is within 20 degrees of the ambient temperature. For example, if the dew point is 65 degrees and it's 80 degrees in your spray area, don't spray unless you use retarder. You need more than a twenty degree difference between the dew point and temperature to be safe.

As the solvents in lacquer evaporate, they have a cooling effect on the surface they're sprayed on (put a few drops of isopropyl alcohol on the back of your hand to feel the effect). The cooling effect can be as much as twenty degrees. If you cool the surface down below the dew point, water will condense on the surface and you'll get blushing the milky white look in the lacquer/shellac.

Also make sure the piece you're spraying is the same temperature as the environment where you're spraying. I once made the mistake of taking a piece from an air conditioned space and spraying it in the outdoor heat. The piece was a lot cooler than the outdoor temperature and the finish blushed almost instantly. In order to spray lacquer in high humidity, you'll need to add lacquer retarder. Lacquer retarder is a slowly evaporating solvent (thinner) that lets the moisture escape from the lacquer before it dries. Only use a small amount of lacquer retarder in place of the regular lacquer thinner. Use the same brand of retarder as the lacquer you're spraying and only use as much as the manufacturer recommends. For example, if you usually thin the lacquer 15% with lacquer thinner, and the manufacturer recommends 5% retarder, switch to 10% lacquer thinner and 5% lacquer retarder (15% total thinning as usual). Adding lacquer retarder causes the lacquer to dry more slowly than usual. Spray your coats a little lighter to avoid runs and sags and allow more time between coats.

From contributor A:
You may also want to check, and then drain your compressor, air lines, and the bleeder valves, and the hoses to the gun. This problem can come from condensation in the compressor.

From contributor B:
Also, too much sanding sealer can cloud a finish.

From contributor C:
Also check the last filter on your air line and make certain that it will also remove water vapor. These go about $2-300. I was getting water spotting on my finishes and after the filter change they are gone.

From the original questioner:
I appreciate the advice. I actually used one of those very cheap disposable in-line air filters which seemed to do well to keep any moisture or condensation out of the gun. I called the manufacturer and they gave me the same advice that you did. It has been a tough week I experienced a bad case of fisheye for the first time and then this blushing problem. I have been spraying finish for along time out of necessity and have never had this happen.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?

Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Finishing

  • KnowledgeBase: Finishing: General Wood Finishing

    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.

    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2016 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB

  • WOODWEB - the leading resource for professional woodworkers

      Home » Knowledge Base » Knowledge Base Article