Today's
Sponsors:


BetterVacuumcups.com

Biesse America

Biewer Lumber

Binks

Black Bros. Co.

Blackhawk Machinery

Briquetting Solutions by Sunomi LLC

Brown Wood Products Co.

Business Management Solutions

Byrd Tool

C.R. Onsrud

Cab Parts

Cabinet Door Service Co.

Cabinet Pro

CabinetCRUNCHER Cutlist & 3D Cabinet Design Software

Cabinetmakers Association

CADCABINETS.COM

CADCode

Cag Lumber

Cantek America

Carolina Woodworking Consultants

Carter Products

Carving Technologies

Castle

Catskill Timber Industries

Charles G.G. Schmidt Co.

Chicago Dowel Company, Inc.

Clear Lake Lumber

CNC Parts Dept.

1-800-Cabinets.com

2Sand.com

3M Corporation

A O M Spray Equipment

Abrasive Resource

Accu-Router, Inc.

AceCo Precision Wood Tooling

Activa

Air Handling Systems

Alan McIlvain Company

Algoma Lumber Co.

All Star Adhesives

Alliance Millsoft

Allied Machinery Inc.

AllRout

Amana Tool

Ameitech South

American Fabric Filter Co.

American Institute of Building Design

American National Woodworking Knife

American Rotary Converters

Andreou Machinery

ANEST IWATA USA, Inc.

Antique Beams and Boards

Antique Building Materials

Anver Corporation

Apollo Sprayers Inc.

Arbor Processing Inc.

Architectural Elements

ArtCam

ATEMAG

Atlantic Machinery Corp.

Auton Motorized Systems

AWFS

B.H. Davis Company

Bailey's Inc.

Baker Products

Banks Hardwoods

Barn Detail

Barn Door Lumber

BC Wood Specialties Group

BeamsRUS

Beaver Tools

Benz Incorporated

Best Cabinets




Best preparation for bent ash       Dr. Gene advises a fishing-net maker on the best ways to prepare ash for bending into frames for his products. 1998.

by Professor Gene Wengert

Q.
I am in need of some technical support related to the bending of air dried ASH strips. The strips are used in the manufacture of the hoop portion of small, handheld trout fishing nets. The strips are approximately 3/8" x 1" x 54" and are to be bent to a radius of 5-6 inches.

I have had good and bad success in the steambending process and am of course interested in eliminating as much of the bad as possible.

Specific questions would then be:

1. Would the best results be achieved by using quarter sawn as opposed to flat sawn wood?

2. What does one ask for to avoid pin knots and even larger knots, which of course create local crossgrain which in turn encourages breakage during the steam bending process? I seem to receive one good batch of wood and then another which has a very high percentage of breakage. Each time the wood grade is noted as FAS...?

3. What is the best moisture content to have? And after the moisture content decreases from sitting in the shop for a period of time will the bending success decrease?

A.
1. Results would be better with quartersawn.

2. FAS grade does not permit very many knots--the piece of lumber must be perfectly clear on the worst face in one or two areas that total 83% of the piece minimum! It sounds like you are not getting FAS if you find pin knots, etc.

3. Moisture content is the most important variable that governs success. For a gentle bend, we would suggest 16% MC or higher (up to 25%). For severe bends, 22 to 28% MC. The next most important factor is steaming time and temperature--always steam with saturated steam too.

Professor Gene Wengert is Extension Specialist in Wood Processing at the Department of Forestry, University of Wisconsin-Madison.

Click on Wood Doctor Archives to peruse past answers.

If you would like to obtain a copy of "The Wood Doctor's Rx", visit the Wood Education and Resource Center Web site for more information.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Lumber & Plywood: Buying

  • KnowledgeBase: Primary Processing: Lumber Grading

  • KnowledgeBase: Primary Processing: Sawmilling

  • KnowledgeBase: Wood Engineering: Wood Properties

  • KnowledgeBase: Woodworking Miscellaneous: Woodworking

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.