Today's
Sponsors:


Royce Ayr Cutting Tools

RT Machine Co.

Safety Speed Cut

Sand-Rite Manufacturing

Sandman Products

Sawmill and Woodlot Magazine

Schultz Forming Products

SCM Group USA, Inc.

SCM Group

SCM

Sears Trostel Lumber Co.

Shade Dri

Shomaker Lumber Company

ShopBot

SII Dry Kilns

Silvaris

Simantech

Single Source Cabinet Supplies

SIS Machinery

SK-USA

SketchList

SlipCon USA, Inc.

SnapDragon Associates, LLC

SNX Technologies

South State Machinery

Southeast Tool, Inc.

Sovereign Machine, Inc.

North Pacific Lumber

Northstate Hardwoods

Northtech Machinery

NPO BARS

O'Shea Lumber Company

Old Mississippi Brick and Heart Pine Company

Omnitech Systems

Onsrud Cutter

Open the Door Products

Opti-Sand

Optisol for Project Scheduling

Original Saw Company

Osborne Wood Products

Paragon Enterprises

Patton Cabinet Doors

Peninsula Hardwoods

Penn Sylvan International

People Logic Software Corp.

Pinske Edge

Pioneer Lumber Company

Pioneer Millworks

Plogic Solutions Ltd.

Pond Cove Paint

Porter-Cable

Precision Drive Systems

Premium Specialty Hardwoods

Prime Estimating and Software Services, LLC

Primo Woodworking Machinery

Pro.Woodworker.com

Pro100

Professional Hardware & Supply Co.

Professional Machinery Group

PYTHA

Quality VAKuum Products, Inc.

Quick Machinery Company

Quickscrews International Corporation

QuickScribe

QuikDrawers

R&R Drummond, Inc.

R.A.W.

R.D. Billhofer Company

Rangate

Rawles-Aden Lumber Corp.

RazorGage

Rex Lumber Company

Riethmiller Lumber

Ritter Manufacturing Inc.

Rockler Woodworking and Hardware

Roger Shaw and Associates

Rose Machinery

Routech

RouterCAD




Drying Rewetted Kiln-Dried Lumber       How to render kiln-dried lumber, which has been rewetted due to flooding or excessive humidity, useful once again. 1998.

School of Natural Resources
Department of Forestry

No. 67 - August 1993

by Eugene M. Wengert and Dan Meyer

Lumber is rewetted in two ways: prolonged exposure to high relative humidities, or exposure to liquid water, as is the case with flooding. (Flooded lumber is discussed in the sidebar at the bottom.) Lumber that is rewetted from high humidities usually has surface moisture contents (MC) of 15% to 20% MC, with cores at or above 10% MC. With prompt attention, however, the increase in moisture content will do little damage--lumber is typically left bright and without any new checking. This lumber can quickly and easily be redried to previous conditions, without much risk of staining, checking or warping, using the procedures outlined below.

Redrying Procedures
Step 1. Determine the present, average moisture content of the lumber, MCp, using sample moisture sections and the same oven-drying methods used for standard kiln drying. Sections should be 1-inch long, along the grain, and the full width and thickness of the lumber. Cut sections from at least 12 representative pieces of lumber. Sample from within and on the edges of lumber stacks. Good sampling will assure that the final MC is at the desired level.

Step 2. Stack the lumber with stickers at least 3/4-inches thick, spaced no further than 24-inches on center. Submerged lumber needs to be cleaned prior to stacking. (Note: If part of the lumber stack was submerged and part remained above water, it will be necessary to separate the lumber into two sorts and dry them separately.)

Step 3. Establish the desired final moisture content, MCf.

Step 4. Begin kiln drying as soon as possible after stacking. Long storage after rewetting or after stacking is not recommended due to the risk of fungal staining and insect damage. Set and maintain the initial dry-bulb temperature at 110°F for hard-to-dry species, such as oak, beech and hickory; 120°F for moderately easy to-dry species, such as hard maple and ash; and 130°F, for easy-to-dry species, such as pine, poplar and soft maple. Keep vents closed and spray lines "off."

Step 5. Once the desired kiln temperature is reached (usually within a few hours), set the humidity. The initial EMC should be halfway between MCp and MCf, but never higher than 18%. (Kiln humidity is specified as an EMC (equilibrium moisture content) percentage. Convert EMC to wetbulb temperature, depression or relative humidity as required for your particular equipment.) Maintain this initial condition for approximately 24 hours. Thick, hard-to-dry lumber may require more time at this setting; thin or easy-drying pieces, less.

Step 6. After 24 hours, increase the dry-bulb temperature to 150°F and decrease the EMC to 2% below the desired final moisture content, MCf. (Common sense may dictate a cooler dry-bulb temperature or may suggest a 6- to 8-hour transition period at an intermediate temperature and EMC, before jumping to 150°F.) Continue drying until MCp equals MCf. Stress relief should not be required, but stress checks should be conducted to be certain.

Example
Previously kiln-dried, 4/4 oak lumber is presently at 15% MC. The desired final MC is 7%. After stacking and loading the kiln, maintain the initial dry-bulb temperature at 110°F, and the initial EMC at 11% (halfway between 15% and 7%). After 24 hours, raise the temperature to 130°F and decrease EMC to 8% for 6 to 8 hours. Following this intermediate setting, change the temperature to 150°F and the EMC to 5% for the remainder of the schedule. When the lumber reaches 7% average MC, check for drying stresses in the usual manner.

Redrying Flooded Lumber
Flooded lumber may have surface and core moisture contents at or above 25% MC, especially if the lumber was underwater for more than a few days. Light-colored lumber reaching these moisture levels may develop fungal sap stain and non-fungal gray stain. In addition, there will typically be residual grit on flooded lumber surfaces which quickly dulls knife blades in machining.

As with humidity-soaked lumber, however, fast action will prevent water-soaked lumber from being a total loss. Lumber that has been submerged can easily be redried, using the same procedures outlined above, with only minimal risk of creating new damage--checks or splits--or aggravating pre-existing damage. Fungal stains are hard to eliminate, but delayed redrying will make them worse. Non-fungal surface staining can be removed, in many cases with a mild solution of oxalic acid. A high-pressure spray will rinse most of the heavy deposits from lumber surfaces, and carbide cutting tools will not be affected by any remaining grit. (Note: Although washing with water may aggravate checking, this brief rewetting will usually not do any damage the flood has not already done.

Gene Wengert is Wood Processing Extension Specialist, Dan Meyer is Associate Outreach Specialist, University of Wisconsin-Madison, Department of Forestry, 1630 Linden Drive, Madison, WI 53706

University of Wisconsin-Extension - United States Department of Agriculture - Wisconsin Counties Cooperating and Providing Equal Opportunities in Employment and Programming



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Lumber & Plywood: Storage

  • KnowledgeBase: Primary Processing: Kiln Operation

  • KnowledgeBase: Wood Engineering: Wood Properties

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article