Drying hickory lumber

      Avoiding sticker stain and bugs in hickory lumber. December 12, 2000

I plan to log some hickory trees in the next couple of weeks and mill them into lumber. Is hickory susceptible to sticker stain? I will shed dry until next spring, when Ill put it in a solar kiln. When I cut hickory for firewood the hickory worms attack it and there will always be piles of sawdust under the firewood pile. Will hickory worms work on lumber?

Forum Responses
We have cut some hickory and it does stain from the stickers if you use anything but cottonwood. We have some more logs to cut soon and they may not be any good as I see worm holes in the bark.

I have experience with 2000+ bf of hickory and it was stickered with dry pine firring strips, with no resulting sticker stain.

Hickory will turn different colors depending on the speed of drying. So, with stickers that are wet, you will see stain. If the wood between the stickers dries faster than the wood under the stickers, you will see stain. If the logs are old (4 weeks of warm weather), then color differences will be enhanced when drying rates are different.

Insect damage is always a risk when they are around. However, all except termites and lyctid powder post will not be present in dry lumber--so dry it ASAP.

Gene Wengert, forum technical expert

Powder post beetles love hickory and ash. Before I would sticker the green hickory, Id treat the lumber with an approved insecticide for powder beetle control. Stack your lumber properly outside with protection to get quicker drying from the outside winds. Don't forget to seal the ends of your lumber. In a few months, move the lumber pile(s) inside your shed.

The powderpost beetle in ash and hickory is not the same one that gets into dry lumber. In green lumber it is the anobiid beetle; in dry, the lyctid. Small holes in green lumber might be due to the ambrosia beetle, but the anobiid beetle is larger than the lyctid by an 1/8 inch.

Ambrosia beetles can be controlled by good yard sanitation (clean up the old wood, sawdust, etc.). Likewise for anobiid.

Gene Wengert, forum technical advisor

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?

Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Primary Processing

  • KnowledgeBase: Primary Processing: Air Drying Lumber

  • KnowledgeBase: Primary Processing: Kiln Operation

  • KnowledgeBase: Knowledge Base

    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.

    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2016 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB

  • WOODWEB - the leading resource for professional woodworkers

      Home » Knowledge Base » Knowledge Base Article