I will be the first to admit that I have a lot learn when it comes to matching stain colors. In this case, I have two pine doors that I had outsourced which I am finishing myself. The doors are to be color matched, as close as possible, with some existing cabinetry in a kitchen. I took a sample door with me to a paint store and matched, (so I thought), a dark walnut color to the sample.

After the doors were stained, I noticed that they were way too dark. I have tried everything, (peroxide wood bleach, etc.), in my attempt to lighten up the doors. Ordering another set of doors is not an option at this point and I am quickly approaching the deadline for the job. Any help would be appreciated.

Forum Responses
(Finishing Forum)
From contributor M:
Sand the doors back down to bare wood and start over. This probably isn’t what you wanted to hear, but it’s probably the only solution for too dark. Cut your stain next time around, and make samples before you stain the doors.



From contributor C:
You never mentioned it, but what’s the type of stain? Meanwhile, I would recommend trying some household bleach.


From contributor C:
Have you tried lacquer thinner, or acetone? I am assuming that this is a pigment stain. It may be enough to cut the color so that you can thin the stain and reapply.


From the original questioner:
I used a dark walnut Varathane penetrating stain. I guess I'll have to just knuckle down and accept the fact that I'll have to painstakingly sand the doors down to bare wood.


From contributor C:
To the original questioner: Was it just a stain, or a stain that is mixed into the Varathane? If it was is mixed into the Varthane, then you first must use a paint remover to take off the Varathane. Bleaching would not help, you first need to remove the Varathane to get to the stain. In some cases the stain may come off with the stripper.


From contributor G:
I've had good results with paint/varnish remover, followed by lacquer thinner. As mentioned above, the remover takes off the topcoat, and the lacquer lightens the stain. Be generous with thinner, have plenty of rags, good respirator, ventilation, etc., and keep wiping down the stain with the LT along the grain in long strokes.


From the original questioner:
Varathane is just the brand name. They have a full array of penetrating stains. This is what I used. I didn't use their finishing product, (i.e., varnish, etc.). All that was applied was the stain only.


From contributor C:
If you only applied a stain, did you try any of these solvents - Acetone, lacquer thinners, lacquer thinners and alcohol, Toulene or Xylene? Do you know what type of stain it is? Look at the label, it should tell you what solvent to use for cleaning up.


From contributor S:
To contributor C: Wouldn't you guess that it is a pigmented oil? Do you know a good way to test?


From contributor C:
To contributor S: Today, just about all of the organic and in-organic pigmented colorants are ground in one of the many synthetic alkyds. Changes are either Toulene or Xylene, or lacquer thinners should do it. Acetone has the highest solvent strength of all these solvents. I'm not really familiar with this stain - it could be part dye and pigments.


From contributor R:
Chlorine bleach will remove most dyes, though it might require several applications. Swimming pool chlorine is stronger and will work faster. For pigments, sometimes the stains own clear stain base will remove a fair amount of pigment. As others have stated try your various solvents, however in most cases I think it is the scrubbing action more than the solvent that is removing the pigment. Sanding is usually the last resort and often the most effective.


From contributor D:
When trying to go from dark to light, before you strip the project and start over, try toning with a yellow toner. I prefer pigmented toners; either French yellow ochre or a chromium yellow. This is the only way I know to try to go from dark to light. If this does not work for the project, you are trying to save it may work for the next project that you need to save. Then, you could always go the last resort and trip and start over.

I place no stock in letting a paint store match a color for stained wood. They match opaque colors. Stained woods have many colors in them. You need to match the look of the stained wood using stains that are in the family of colors that you want. That is a lot different than matching an opaque color.

Stained woods are a combination of the coloring steps and materials plus the wood. It is the various steps and application of those coloring steps which bring you the final coloring results.



From contributor H:
I've sanded doors many times and it really doesn't take long. I would recommend that next time you spray your stains on in very light coats (with lots of air and very little fluid), and sneak up on the right darkness. Each coat should dry instantly. Thin the stain between 50% and 75% and try it on a sample board first.

Keep your original sample close by. I use a gun of thinned dark walnut and another gun with thinned early American to match lots of different tones. The early American warms it up and has more red, and that helps dark walnut, which has more green.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Finishing

  • KnowledgeBase: Finishing: Refinishing


    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2018 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB











  • WOODWEB - the leading resource for professional woodworkers


      Home » Knowledge Base » Knowledge Base Article