Question
It seems that 1/2" OSB has replaced 1/2" CDX as sheathing for most residential construction. In the interest of getting rid of my stacks of excess, lower quality pine boards, I am considering going old school and using it to sheath a spec house next spring.
My questions are:
1) Would board sheathing make a house more susceptible to mice?
2) Would putting a shiplap on the rough-cut boards eliminate the need for let-in bracing or diagonal sheathing?
3) Is there a potential market for board sheathing for people who don't want exposure to outgassing of OSB and Advantek?
Forum Responses
(Sawing and Drying Forum)
From Professor Gene Wengert, forum technical advisor:
The plywood or OSB sheathing provides a much more rigid structure than board sheathing. As most houses use poly vapor barriers on the inside, the off-gas from wall sheathing is not a factor.
1. Properly done, I cannot see a difference.
2. Check with building code people to see what they will accept. At the least, I think you should use OSB for the corners. The higher cost of installation for boards would seem to make this an expensive way to get rid of your surplus.
3. I doubt that this is an issue for a home buyer.
To answer your question about the pine siding, that is exactly what I am doing. I am milling the wood here in Florida on my Timberking B-20 and hauling it to Colorado. What I have done is sheet it with OSB, cover that with Tyvek and put 8" wide SYP boards over that, then 2" battens.
Looks good and so far is weathering really nice. To speed up the weathering I will coat the exterior wood with a solution made from vinegar and steel shavings for that really old looking effect.
The original question was the use of pine boards for sheathing and not siding. My response is in reference to sheathing, and not siding.
I would recommend surfacing the material for uniform thickness. Otherwise I would think you'll be fighting the rough sawn variances throughout the siding process. Also, some sort of "coverage" joint - shiplap or tongue and groove - should be used if possible to prevent gaps at the joints as the material shrinks and/or swells.
And most importantly, if applied diagonally, book match the application on a wall rather than applying in only one direction. When applied in one direction, the entire house will twist as the sheathing dries. There are a number of old texts I recall reading that were adamant about this.
Building "green" here means the boards have not traveled over 100 miles and are not glued together. Yes, it takes longer and may cost a bit more, but then better things usually do.
Common Lumber Name | A | B | C |
Hardwoods | |||
Alder, Red | 9.9 | 19.2 | 2506 |
Apple | 10.9 | 31.7 | 4132 |
Ash, Black | 9.3 | 23.4 | 4132 |
Ash, Green | 14.3 | 27.6 | 3590 |
Aspen, Bigtooth | 10.3 | 18.7 | 2439 |
Aspen, Quaking | 10.3 | 18.2 | 2373 |
Basswood | 6.2 | 16.6 | 2174 |
Beech, American | 8.9 | 29.1 | 3793 |
Birch, Paper | 8.8 | 25.0 | 3260 |
Birch, Sweet | 11.9 | 31.2 | 4065 |
Birch, Yellow | 9.2 | 28.6 | 3723 |
Buckeye | 8.9 | 17.2 | 2235 |
Butternut | 11.3 | 18.7 | 2440 |
Cherry | 13.8 | 24.4 | 3184 |
Chesnut, American | 11.6 | 20.8 | 2708 |
Cottonwood | 8.5 | 16.1 | 2102 |
Dogwood | 6.8 | 33.3 | 4331 |
Elm, American | 10.2 | 23.9 | 3116 |
Elm, Rock | 12.2 | 29.6 | 3860 |
Elm, slippery | 11.5 | 25.0 | 3251 |
Hackberry | 11.8 | 25.5 | 3319 |
Hickory, Bitternut (Pecan) | 14.7 | 31.2 | 4062 |
Hickory (True) | |||
Hickory, Mockernut | 9.1 | 33.3 | 4332 |
Hickory, Pignut | 9.3 | 34.3 | 4332 |
Hickory, Shagbark | 10.9 | 33.3 | 4333 |
Hickory, Shellbark | 6.6 | 32.2 | 4195 |
Holly, American | 8.3 | 26.0 | 3387 |
Hophornbeam, Eastern | 7.9 | 32.8 | 4266 |
Laurel, California | 15.1 | 26.5 | 3456 |
Locust, Black | 21.2 | 34.3 | 4470 |
Madrone, Pacific | 7.8 | 30.2 | 3925 |
Maple (Soft) | |||
Maple, Bigleaf | 12.8 | 22.9 | 2980 |
Maple, Red | 13.1 | 25.5 | 3318 |
Maple, Silver | 12.4 | 22.9 | 2981 |
Maple (Hard) | |||
Maple, Black | 12.3 | 27.0 | 3523 |
Maple, Sugar | 12.3 | 29.1 | 3793 |
Oak (Red) | |||
Oak, Black | 11.7 | 29.1 | 3792 |
Oak, California black | 16.4 | 26.5 | 3455 |
Oak, Laurel | 6.3 | 29.1 | 3791 |
Oak, Northern red | 13.6 | 29.1 | 3793 |
Oak, Pin | 13.0 | 30.2 | 3928 |
Oak, Scarlet | 13.2 | 31.2 | 4065 |
Oak, Southern red | 9.6 | 27.0 | 3520 |
Oak, Water | 10.4 | 29.1 | 3793 |
Oak, Willow | 6.4 | 29.1 | 3790 |
Oak (White) | |||
Oak, Bur | 15.4 | 30.2 | 3928 |
Oak, Chestnut | 10.1 | 29.6 | 3858 |
Oak, Live | 17.5 | 41.6 | 5417 |
Oak, Overcup | 10.7 | 29.6 | 3860 |
Oak, Post | 11.0 | 31.2 | 4063 |
Oak, Swamp chestnut | 10.7 | 31.2 | 4063 |
Oak, White | 10.8 | 31.2 | 4062 |
Persimmon | 7.0 | 33.3 | 4332 |
Sweetgum | 8.9 | 23.9 | 3115 |
Sycamore | 10.7 | 23.9 | 3115 |
Tanoak | 9.0 | 30.2 | 3926 |
Tupelo, Black | 10.4 | 23.9 | 3116 |
Tupelo, Water | 12.4 | 23.9 | 3115 |
Walnut | 13.4 | 26.5 | 3454 |
Willow, Black | 8.6 | 18.7 | 2438 |
Yellow-poplar | 10.6 | 20.8 | 2708 |
Common Lumber Name | A | B | C |
Softwoods | |||
Baldcypress | 13.2 | 21.9 | 2844 |
Cedar, Alaska | 14.4 | 21.9 | 2844 |
Cedar, Atlantic white | 10.9 | 16.1 | 2100 |
Cedar, eastern red | 16.4 | 22.9 | 2981 |
Cedar, Incense | 13.1 | 18.2 | 2371 |
Cedar, Northern white | 11.1 | 15.1 | 1964 |
Cedar, Port-Orford | 12.6 | 20.2 | 2641 |
Cedar, Western red | 12.2 | 16.1 | 2100 |
Douglas-fir, Coast type | 12.3 | 23.4 | 3049 |
Douglas-fir, Interior west | 13.2 | 23.9 | 3116 |
Douglas-fir, Interior north | 14.0 | 23.4 | 3048 |
Fir, Balsam | 9.9 | 17.2 | 2236 |
Fir, California red | 10.6 | 18.7 | 2437 |
Fir, Grand | 10.7 | 18.2 | 2371 |
Fir, Noble | 10.1 | 19.2 | 2507 |
Fir, Pacific silver | 10.4 | 20.8 | 2711 |
Fir, Subalpine | 10.5 | 16.1 | 2101 |
Fir, White | 12.2 | 19.2 | 2506 |
Hemlock, Eastern | 12.6 | 19.8 | 2573 |
Hemlock, Western | 11.5 | 21.8 | 2847 |
Larch, Western | 11.3 | 25.0 | 3251 |
Pine, Eastern white | 12.3 | 17.7 | 2303 |
Pine, Lodgepole | 11.5 | 19.8 | 2576 |
Pine, Ponderosa | 12.6 | 19.8 | 2573 |
Pine, Red | 12.2 | 21.3 | 2777 |
Southern yellow group | |||
Pine, Loblolly | 12.9 | 24.4 | 3183 |
Pine, Longleaf | 15.0 | 28.1 | 3658 |
Pine, Shortleaf | 12.9 | 24.4 | 3183 |
Pine, Sugar | 12.6 | 17.7 | 2302 |
Pine, Western white | 10.0 | 18.2 | 2370 |
Redwood, Old growth | 14.9 | 19.8 | 2573 |
Redwood, Second growth | 13.2 | 17.7 | 2302 |
Spruce, Black | 11.3 | 19.8 | 2575 |
Spruce, Engelmann | 10.0 | 17.2 | 2234 |
Spruce, Red | 10.6 | 19.2 | 2506 |
Spruce, Sitka | 10.8 | 19.2 | 2506 |
Tamarack | 12.0 | 25.5 | 3318 |