Today's
Sponsors:


BetterVacuumcups.com

Biesse America

Biewer Lumber

Binks

Black Bros. Co.

Blackhawk Machinery

Briquetting Solutions by Sunomi LLC

Brown Wood Products Co.

Business Management Solutions

Byrd Tool

C.R. Onsrud

Cab Parts

Cabinet Door Service Co.

Cabinet Pro

CabinetCRUNCHER Cutlist & 3D Cabinet Design Software

Cabinetmakers Association

CADCABINETS.COM

CADCode

Cag Lumber

Cantek America

Carolina Woodworking Consultants

Carter Products

Carving Technologies

Castle

Catskill Timber Industries

Charles G.G. Schmidt Co.

Chicago Dowel Company, Inc.

Clear Lake Lumber

CNC Parts Dept.

1-800-Cabinets.com

2Sand.com

3M Corporation

A O M Spray Equipment

Abrasive Resource

Accu-Router, Inc.

AceCo Precision Wood Tooling

Activa

Air Handling Systems

Alan McIlvain Company

Algoma Lumber Co.

All Star Adhesives

Alliance Millsoft

Allied Machinery Inc.

AllRout

Amana Tool

Ameitech South

American Fabric Filter Co.

American Institute of Building Design

American National Woodworking Knife

American Rotary Converters

Andreou Machinery

ANEST IWATA USA, Inc.

Antique Beams and Boards

Antique Building Materials

Anver Corporation

Apollo Sprayers Inc.

Arbor Processing Inc.

Architectural Elements

ArtCam

ATEMAG

Atlantic Machinery Corp.

Auton Motorized Systems

AWFS

B.H. Davis Company

Bailey's Inc.

Baker Products

Banks Hardwoods

Barn Detail

Barn Door Lumber

BC Wood Specialties Group

BeamsRUS

Beaver Tools

Benz Incorporated

Best Cabinets




Radius of Convex Wall       Formulas for calculating this measurement. May 19, 2004

Question
I need to do a 1x12 shelf for a closet that has a convex (outward) curve. I want to determine the radius for the wall so I can set up a trammel for my router to cut the inner and outer edges.

I could probably just scribe a piece of paper along the wall at floor level and then measure arc length and cord length, but I am interested in other possible methods.

Forum Responses
(Architectural Woodworking Forum)
From contributor H:
I suggest scribing a pattern rather than using another method. I'm betting the wall isn't a perfect arc, so unless you use a pattern, you could have gaps.



From contributor S:
R = radius, H = height from intersection of chord length to apex of radius. X = chord length. A little confusing but once you understand it, it works perfect every time. This should get you close, then just a little scribe to fit to variations of sheetrock wall.




From contributor C:
I think this is basically the same as the formula above, but possibly a simpler version. L = 1/2 of chord length, Q = 1/4 of chord length. Knowing how to calculate radiuses from only a segment of a circle can be a very useful tool, although I would probably just scribe if given the situation you presented.




From contributor A:
Because it is a convex wall, he cannot establish a chord length or height from the chord to the apex of the arch.

I suppose you would have to make a U-shaped jig - two legs the same length screwed (perfectly square) to a third board. Knowing the length of the chord board and the two jig legs, it could be placed against the wall, the remaining distance from 1/2 the cord to the wall subtracted from the jig leg length, and then the necessary math could be done. I'm just shooting from the hip here… what do you think?
From the original questioner:
Thank you for the calculations. However, since this is a convex curve, I was looking for a method to calculate the radius when the cord length and height of the arc are not known.

I realize I could put a piece of paper on the floor and cut out the arc and hence obtain the cord length and height of the arc. Just wondering if someone has another method for derving the radius on a convex curve that might be a little quicker than laying down paper and cutting out a template.




From contributor F:
Make sure that both of the lines labeled B are parallel. Make sure that the line A is perpendicular to B

At the center of line A, draw a perpendicular line and call that B2.

Measure lines A, B and B2.

Line B - B2 = H
Radius = ((A^2) + (H^2))/2*H

A-




From contributor S:
Yes, you can use my formula. Refer to the photo below.

Place a level, the longest that will fit, against wall. Then measure to wall at each end square. When both ends measure the same, this is = H. Now let's say, for the sake of argument, that level is 48" long and the equal dimension at both ends is 6". You now have both dimensions to complete formula.

X = 48"
H = 6"

48/2 = 24
24x24 = 576

6x6 = 36

576+36 = 612

2x6 = 12

612/6 = 102

102" is your radius.

I realize you can't measure chord length as is. You need straight edge across face and to measure squarely off ends. The longer edge you can fit, the better accuracy you will have.




From contributor R:
The radius of the wall is very likely not true. If you don't want to deal with gaps, make a template. All the math in the world will not be worth the trouble on an irregular shaped wall. In a perfect world, any one of the math problems above would probably work for you, but if the wall was perfect you wouldn't be asking this question. If you do make a template, do not make it at the floor level! Make your template at the exact elevation of the installation.


From contributor K:
Is your convex wall created by a circular staircase? If so, call the stair builder and ask about the outside radius of the convex stringer. That will put you in the ballpark. You're going to need to scribe anyway!

However, thank you for the shop math lesson. Do any of you know how to lay out an ellipse with two sticks, two runner sticks, two nails, and a pencil? Have seen this done before, but forget how exactly the math goes. (I need to recall this or learn of another layout method because I have an upcoming project that calls for it.)



From contributor A:
The method of laying out an ellipse you describe is illustrated and explained in the book Circular Work in Carpentry and Joinery by George Collings. It is published by Linden Publishing Co. in Fresno Ca. This is a good book to have. It gives the formulas described above and also practical ways to get the job done.

I still think it's easier to make the jig I described earlier to determine the chord length and apex than to draw a series of lines on the floor every time or try to get a level to stay in place - and what if it's a finished floor? Not only that in my experience the reference points are more accurate this way.



From contributor Y:
You could search the Knowledge Base for the discussion last year on the same topic in which was described the 'tick stick' method. No math, no paper, absolutely precise, and when you are done you have your template to run your pattern bit against. It has been used by shipwrights for centuries. Of course those guys didn't have routers with pattern bits.


From contributor F:
Contributor S's and my formula should be the same. There was a mistake in mine. It should be:

Radius = (((A/2)^2) + (H^2))/2*H

A-



From the original questioner:
Thanks for all of the great methods for finding the radius of the convex curve. I'm really impressed with the quality of knowledge I gained here. Below I have described how I used all the suggestions.

Shelf inner and outer radius:
I like the jig idea and will actually make a collapsible one for future use. In the interim, I used an 8 foot level, measurement techniques, and formulas from the postings to gain the radius. I then drew both the inner radius (+1/4") and the outer radius (+1/2") out on the 4x8 MDF sheet I was going to use for shelving, and cut out the rough shape. I mounted this rough shape on cleats at the proposed shelf height and scribed the exact fit (yes, the curved walls had waves) with a pencil, using a 1" fender washer to gain the inner curve. I then re-cut the rough shelf with the scribed edge for the inner radius using a jig saw. I completed the outer radius with a router and trammel to gain a perfect curve for the outer shelf edge.

It fits and looks great! Thanks again for all the advice. What a great forum!



The comments below were added after this Forum discussion was archived as a Knowledge Base article (add your comment).

Comment from contributor D:
Two words - "flexible curve". Rockler sells a product that can bend to as small as a 1" radius. You form it to your wall or whatever you need, it maintains the shape, then you transfer as needed. The only drawback is the longest one you can get is 36".



The comments below were added after this Forum discussion was archived as a Knowledge Base article (add your comment).



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Architectural Millwork

  • KnowledgeBase: Architectural Millwork: General

  • KnowledgeBase: Business: Estimating/Accounting/Profitability

  • KnowledgeBase: Business: Project Management

  • KnowledgeBase: Cabinetmaking

  • KnowledgeBase: Cabinetmaking: Cabinet Design

  • KnowledgeBase: Cabinetmaking: General

  • KnowledgeBase: Furniture

  • KnowledgeBase: Furniture: Furniture Design

  • KnowledgeBase: Woodworking Miscellaneous




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article