      Looking for a fix for an edge-banding failure on a built-in desk. April 20, 2011

I have a problem with a recent edgeband that I did on a job. It's on a very large desk cubicle that I built for an architectural firm. It is on the face of the desk, the top being birch plywood. I applied contact cement and birch veneer and I am very unhappy with its durability. I am considering removing the veneer and applying solid maple instead. Any comments?

Forum Responses
(Laminate and Solid Surface Forum)
From contributor L:
Contact cement is your problem. You should be using some sort of a rigid glue - TiteBond, UniBond or something that dries hard.

From the original questioner:
Right. That makes sense. After removing the veneer and stripping the surface, will the bond still be strong after reapplying?

One issue I just thought of... The units I built are in place and the glues that you suggest are slow setting. Without a fast setting glue, how would I successfully apply the veneer?

From the original questioner:
I'm scraping the veneer and applying a hardwood face with 3/16" maple to match the birch top and solve the defect of separation and durability at the miter corners. This gives me the ability to further break the edge for more comfort and a better look. I believe this will be my best bet.

From contributor P:
They make a double sided tape that I hear works pretty well. I use contact cement for edging (if I can't use the edgebander) all the time with no problems. Don't do this with sheet veneer or you will have lots of trouble.

From the original questioner:
Well, the edge of the desk is 1 3/8" thick. Is there only one size to the tape? My other issue is making a comfortable desk edge. The hardwood thickness will help with that because I can't take down the plywood edge without going through the veneer.

From contributor P:
They make it to order, so any size you want. I would use the solid wood for that situation.

From the original questioner:
I thought it to be more surefire. And it would look great. But I will keep the tape in mind for the future. I think I used something similar recently on a job. It was a large peal-away sheet I used on some cabinets.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?

Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Adhesives, Gluing and Laminating

  • KnowledgeBase: Adhesives, Gluing and Laminating: Glues and Bonding Agents

  • KnowledgeBase: Cabinetmaking

  • KnowledgeBase: Cabinetmaking: Installation

  • KnowledgeBase: Furniture

  • KnowledgeBase: Furniture: Furniture Repairs

    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.

    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2017 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB

  • WOODWEB - the leading resource for professional woodworkers

      Home » Knowledge Base » Knowledge Base Article