Question
WOODWEB Member:
I'm working on a Corian countertop for an island that is 52" x 96". In addition to the seam of the 2 sheets of Corian, I'll be miterfolding the edges all the way around so the top appears to be 3-1/2" thick.

I used to work with Swanstone several years ago and we always used to put a spline in the joint when we seamed two sheets together. Is this necessary? I watched this video and they aren't using a spline and the joint shows incredible strength.

I made a test piece with Corian without a spline and I was able to break the joint without much effort. I only used spring clamps but I thought that should have been adequate. Has my adhesive gone bad? It has been stored above 70 degrees and it's about 6 months old.

Forum Responses
(Laminate and Solid Surface Forum)
From contributor J:
We have been doing Corian and other solid surface for many years. For doing a spline in the joint, I would not recommend that at all and would maybe void the warranty. I would use a wavy edge bit for the seam, make more glue contact, and do a 4'' seam plate on the underside. Always cut the plate at a 45 angle. Check the glue, as we have been having some problems with the hardener not coming out in older tubes. Purge it before you install the tip; it seems to set up in the tube and we have to take a small drill bit and open the hole up.



From contributor A:
I have to agree with contributor J, with the possible exception of the wavy edge bit - it's not really necessary. A good straight edge is fine, but the advice of using a seam block and purging the adhesive tube is 100% correct. You should also be cleaning the contact areas with denatured alcohol before applying the adhesive. Dupont has some very specific requirements for fabricating Corian, and it is best to follow them.


From contributor P:
Thanks for the responses. I understand the seam block - but I'm not sure what you mean by cutting it at 45 degrees.

Also, I'm wondering if my adhesive has gone bad. It says not to store it above 70 degrees, and it was 95 in the shop a few weeks ago - although when I'm actually gluing, it's only about 75 degrees. Have you ever had adhesive go bad or is it probably just a mixing problem (maybe the hardener isn't getting released in the right ratio)?

Thanks again - I'm fairly new to solid surface. I am not a licensed Corian installer because I'm just doing commercial work, which they don't warranty anyway.



From contributor J:
The seam plates we do are ripped on a 45 degree on the table saw, then glued to the underside of the top. I have no problem with hot weather storage in the tubes. My main problem is that in the tubes, the hardener has been setting up. I always put the grey cap that the tubes come with back on after every use. I use both the 470 and 50 ml, but I like the small ones better. Out of date glue can be a big problem, so check the date on the glue! I do not use if it's out of date.


From contributor E:
I agree with the other comments, except they never said anything about roughing the seam with 80 grit sandpaper, which really adds strength for me. Also, if you don't have seam clamps, a cheap alternative is to use C clamps and bungee straps to keep an even pressure on the seam. Key to a seam for me is even pressure, denatured alcohol, scuff with sandpaper. Also use metal tape under the seam and have some support behind the seam when you glue them. I set my tops up on top of some MDF or particleboard until it's ready to build up.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Laminates and Solid Surfacing

  • KnowledgeBase: Laminates & Solid Surfacing: Fabrication Techniques


    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2018 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB











  • WOODWEB - the leading resource for professional woodworkers


      Home » Knowledge Base » Knowledge Base Article