Today's
Sponsors:


Finish Systems

Firth Maple Products

FORDAQ

FormWood Industries

Freeborn Tool Company

Fuhr International

Fuji Spray

Gabbiani Machine

Gary M. Katz

Global Hardwood Flooring

Glue Machinery Corporation

Goby Walnut Products

Graco, Inc.

Granite Road

Grayson Ferguson Woodworking Inc.

Great Lakes Kiln Drying Association

GreCon

GUHDO

Hanson and Leja Lumber Company

Hardwood Council

Hardwood Store of N.C. Inc.

Heartwoods, LLC

Her-Saf

Hermance Machine Company

High Point Grinding - Total Saw Solutions

Historical Plus Wood

CNCROUTERSTORE.com

CNT Motion Systems

Colonial Saw

Construction Programs and Results

Cook's Saw Mfg.

COOLwoodworkingstuff.com

Country Saw & Knife, Inc.

Courmatt International Inc.

CP Adhesives

CSH Custom Service Hardware Inc.

CTS Manufacturing Inc.

CustomMade.com

Cutlist Plus

D.S. Brown Machinery

Dancer Lumber

Delle Vedove USA, Inc.

Delmac Machinery Group

Delta

Denray Machine

DeVilbiss

Dispoz-A-Blade

Diversi-Tech

DMC

DODDS

Don Hall & Associates

Donald Dean and Sons

Durable Wood Products

E.W. Tooling Inc.

Eagle Machinery and Repair Co.

ECabinet Systems

Edge-It Edgebanding

Edwards Wood Products

Electrophysics

Elias Woodwork & Manufacturing

Elkom North America

Emerald Hardwood Floors

Endeavor Hardwoods

EnRoute WOOD

ETemplate Digital Measuring

ETK International

EX-FACTORY

Excel Dowel and Wood Products Inc.

Extrema Machinery

ez-Router

FastCap




Shrinkage allowances for red oak       Estimating radial and tangential shrinkage when drying red oak to 12 to 14 percent MC. 1998.

by Professor Gene Wengert

Q.
I am going to slice 6/4 green northern red-oak (quercus rubra) to make flooring wear layers for a Swedish laminated flooring company to a thickness of .189" x 8-3/4" in width, and then dry these wear layers to 12-14% or so.

My question is, with a rather gentle forced-air kiln at a temperature of approx 95 degrees F, how much shrinkage should I allow for radially and tangentialy as well?

Also, as we are in Idaho, we use a lot of white spruce stickers. This should hopefully not stain the wood. Would spruce be the desired sticker-material?

A.
The standard shrinkage values for northern red oak from green to 12% are averages (so half the pieces will shrink slightly more) and also vary for each species of red oak. To be 100% safe, I would expect 9% tangential and 4.5% radial. This means that all pieces will actually be too wide, so you may wish to save a little wood and make them 4% and 7.5% larger, which means that once in a while you will have a narrow piece, but not very often.

No problem with the spruce sticks if they are dry.

Professor Gene Wengert is Extension Specialist in Wood Processing at the Department of Forestry, University of Wisconsin-Madison.

Click on Wood Doctor Archives to peruse past answers.

If you would like to obtain a copy of "The Wood Doctor's Rx", visit the Wood Education and Resource Center Web site for more information.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Architectural Millwork: Flooring

  • KnowledgeBase: Laminates & Solid Surfacing: Materials

  • KnowledgeBase: Primary Processing: Kiln Operation

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.