Today's
Sponsors:


Royce Ayr Cutting Tools

RT Machine Co.

Safety Speed Cut

Sand-Rite Manufacturing

Sandman Products

Sawmill and Woodlot Magazine

Schultz Forming Products

SCM Group USA, Inc.

SCM Group

SCM

Sears Trostel Lumber Co.

Shade Dri

Shomaker Lumber Company

ShopBot

SII Dry Kilns

Silvaris

Simantech

Single Source Cabinet Supplies

SIS Machinery

SK-USA

SketchList

SlipCon USA, Inc.

SnapDragon Associates, LLC

SNX Technologies

South State Machinery

Southeast Tool, Inc.

Sovereign Machine, Inc.

North Pacific Lumber

Northstate Hardwoods

Northtech Machinery

NPO BARS

O'Shea Lumber Company

Old Mississippi Brick and Heart Pine Company

Omnitech Systems

Onsrud Cutter

Open the Door Products

Opti-Sand

Optisol for Project Scheduling

Original Saw Company

Osborne Wood Products

Paragon Enterprises

Patton Cabinet Doors

Peninsula Hardwoods

Penn Sylvan International

People Logic Software Corp.

Pinske Edge

Pioneer Lumber Company

Pioneer Millworks

Plogic Solutions Ltd.

Pond Cove Paint

Porter-Cable

Precision Drive Systems

Premium Specialty Hardwoods

Prime Estimating and Software Services, LLC

Primo Woodworking Machinery

Pro.Woodworker.com

Pro100

Professional Hardware & Supply Co.

Professional Machinery Group

PYTHA

Quality VAKuum Products, Inc.

Quick Machinery Company

Quickscrews International Corporation

QuickScribe

QuikDrawers

R&R Drummond, Inc.

R.A.W.

R.D. Billhofer Company

Rangate

Rawles-Aden Lumber Corp.

RazorGage

Rex Lumber Company

Riethmiller Lumber

Ritter Manufacturing Inc.

Rockler Woodworking and Hardware

Roger Shaw and Associates

Rose Machinery

Routech

RouterCAD




Thinning Precatalyzed Lacquer       Adding thinner reduces the solids ratio of the mixture; warming it up does not. April 19, 2006

Question
I have been spraying more and have been using Magnalac. I was wondering to what percentage you thin your material? I am using HVLP with a 1.5 tip. Also is there any benefit to moving up to Magnamax?

Forum Responses
(Finishing Forum)
From contributor A:
I thin 10 % - moving up to higher grade lacquer depends on what you are building



From contributor B:
Viscosity is more important than % of thinner. Get and use a viscosity cup and you can fine tune your thinner addition. You can also heat your lacquer to reduce viscosity.


From contributor C:
I've sprayed both Magnalac and Magnamax. There is no comparison. I cannot tell the difference between Magnalac and cheap nitrocellulose snot. Magnamax is a fine product. If Magnamax was removed from the shelf, I'd not use Magnalac - I'd either use Duravar, Krystal, or perhaps switch to Chemcraft's Opticlear.


From contributor D:
Magnalac is thinned with the lacquer thinner mentioned by MLC in their tech sheet.
Contributor B singles in on the only important issue, viscosity. You match the viscosity of the material you are spraying to your needle/nozzle of your spray gun. The thickness of a material is lowered in one of two ways, either by introducing more reducer (thinning) or by raising the temperature of the material. When you raise the temperature of the material you do not lower the percentage of solids by volume. When you reduce the material you do lower the percentage of solids by volume.

Magnalac is way too finicky a material for a lot of us. It does not seem to tolerate going over that dried mil thickness unless you do not mind a finish that shatters. As far as the durability of Magnalac, it is little better than ordinary lacquer. It is a precat, sure, but so what. There are so many other precats that perform so much better than Magnalac after three weeks of crosslinking. Magnamax is just one of them.

My favorite finish is lacquer. Calling it by some gooey name is inaccurate. That label of derision belongs to the many waterbase finishes and only to that part of the game when you need to strip off waterbase.



From contributor C:
I kind of like the gimmicky names for one reason (other than they're easier for me to remember). Customers like gimmicky names. Telling them their $60,000 cabinets are finished in precat lacquer sounds ok to them, but tell them it's Magnamax and it sounds a little more Schwarzenegger.

I'll never understand, though, where Chemcraft came up with "Danspeed" as the name for a conversion varnish. Sounds like "Dan's peed" in a bucket and we slopped it on some cabinets.



From contributor B:
You should love Becker's Bernyl Strong.


From contributor E:
Danspeed is not a conversion varnish. It is a post-catalyzed lacquer

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Finishing

  • KnowledgeBase: Finishing: General Wood Finishing




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.