Today's
Sponsors:


Vintage Wood Products

VortexTool Co. Inc.

VyTek

W. Moore Profiles, Ltd.

W.L. Fuller

Wagner Electronic Products

WalzCraft Industries

WEIMA America, Inc.

Weinig Group - USA

Western Dovetail

Williams and Hussey

Wisconsin Knife Works

WMIA

WMMA

Wood Doctor's Rx, LLC

Wood Technology Inc

Wood-Mizer

WoodCabinetDoors.Com

WoodenBoat

WoodFinder

WoodJobs.com Search Consultants

WoodLINKS

Woodmaster

WoodPlanet Inc.

WoodSprayGuns.com

WOODWEB

Woodworker's Supply/woodworker.com

Woodworker's Directory

Woodworking in America

Wright Timber

Specialtytools.com

Speed Sander

Spink Lumber

Sprayguncaptain.com

Stefani

Steve H. Wall Lumber Co.

Stiles Machinery

Stiles Shop Solutions

Stoneys Hardwoods

Super Source Tooling Inc.

Supergrit Abrasives

Superior Wood Products

T-Tool USA LLC

Target Coatings

TaylorCraft Cabinet Door Company

Techno CNC Routers

Template Services

The Veneer Store

Thermwood Corporation

Tiger Wood Ltd.

TigerStop

TigerwoodDecking.com

TimberKing

Timesavers Inc.

TMS Machinery Sales

Tomlin Architectural Millwork

Tooling on the Web

Toolstoday.com

Top Drawer

Touch Up Solutions LLC

Tractivity

TradeJobPlacement.com

TradeSoft

Trakware Systems Inc.

TRB Flooring Company

Tropical Hardwoods

True North Cedar

Ubidmachinery Inc.

UC Coatings Corp.

Unique Building Supples

Unique Machine & Tool

University of Wisconsin

UWMO Auctions

VacDry Kilns

Vacuum Pressing Systems, Inc.

Vacuumpods.com

Valspar

Vecoplan LLC

Vector Art 3D

Vectric Ltd.

Veneer Systems Inc.




Troubleshooting Bubbles in a Vacuum-Press Veneer Glue-Up       Platen characteristics, veneer issue, or glue quality might be to blame for small bubbles appearing under the veneer. April 7, 2008

Question
I recently built a vacuum pump and bag to do some kitchen door panels. I'm getting about 20lbs of neg pressure from the pump and a good seal in the bag. I'm using various figured veneers and cold press veneer glue onto 1/4" MDF between 3/4 melamine platens. I keep getting bubbles in the veneer - some big, some small, but I'm consistently screwing these panels up. Anyone ever have this happen? I originally thought maybe I was rolling on too much glue, but now am baffled. Maybe bad glue?

Forum Responses
(Adhesive Forum)
From contributor F:
My take is that there no bad glues if it's a PVA and if it flows. What is cold press veneer glue? Urea, PVA, PVA II, or Fast Set as in FSV? Zero in on moisture, is my bet. Urea and FSV work pretty darned good in a bag.



From contributor C:
Bubbles towards the edges can result from the top platen being too big. 3/4 platens shouldn't overhang any edge by more than 1/4". I go for 1/8 to 3/16.


From Jeff Pitcher, forum technical advisor:
I'd be curious to know what the bubbles look like if you slice them open. You can tell a lot by looking at the failed glue area. It may be that you've applied too much glue or it could be contamination or too little glue in those spots. I doubt you're getting 20lbs of pressure, as a vacuum press is only capable of drawing 1 atmosphere of pressure (~14.6 lb/square inch).


From contributor W:
Are your veneers flat and pliable or wrinkled and dry? Raw veneer or prepared on paper or veneer?


From the original questioner:
The glue is not a PVA. The bubbles aren't on the edges, they are exclusively toward the middle. They feel hard but after some time, soften up. The veneer is raw and is figured as well, some are a little lumpy, but not too bad. I've used much worse. As far as the pressure, I don't know the science behind it, but my gauge reads 20 and it cycles back on when it drops to 18 (I have a slight leak at a valve). In my tests it broke melamine and MDF panels that weren't laid flat.


From contributor T:
Are your platens grooved on the outside surfaces? This is to draw out all air. Are your platens bigger than the work piece? If the pressure is forcing an overhanging edge down, it is also not pressing the middle of the panel. If you have an overhanging platen setup and are using filler blocks to fill the open voids, make absolutely sure they are exactly the same thickness as the work piece. Are you taking too long getting it in the bag, allowing the adhesive to skin over?


From contributor T:
I just want to add that when I'm pressing panels I make the platens exactly the same size as the work piece, then pin two of the corners so it doesn't shift. It is guaranteed to press properly this way.


From contributor G:
The bubbles could be a result of the veneer not being uniform in thickness. A 3/4" thick caul will not conform to minor variations. I suggest either using a sheet of rubber between the caul and the veneer, or using a thinner caul. 1/4" thick material will be fine.


From the original questioner:
Well, I pressed up a bunch of panels this weekend, and they all came out fine. I did two things differently than before - I bought some new glue (essentially the same stuff, just new) and used less of it. What was the problem? I suspect it was settled, old glue, but who knows.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Veneer

  • KnowledgeBase: Veneer: Techniques




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article