Today's
Sponsors:


Royce Ayr Cutting Tools

RT Machine Co.

Safety Speed Cut

Sand-Rite Manufacturing

Sandman Products

Sawmill and Woodlot Magazine

Schultz Forming Products

SCM Group USA, Inc.

SCM Group

SCM

Sears Trostel Lumber Co.

Shade Dri

Shomaker Lumber Company

ShopBot

SII Dry Kilns

Silvaris

Simantech

Single Source Cabinet Supplies

SIS Machinery

SK-USA

SketchList

SlipCon USA, Inc.

SnapDragon Associates, LLC

SNX Technologies

South State Machinery

Southeast Tool, Inc.

Sovereign Machine, Inc.

North Pacific Lumber

Northstate Hardwoods

Northtech Machinery

NPO BARS

O'Shea Lumber Company

Old Mississippi Brick and Heart Pine Company

Omnitech Systems

Onsrud Cutter

Open the Door Products

Opti-Sand

Optisol for Project Scheduling

Original Saw Company

Osborne Wood Products

Paragon Enterprises

Patton Cabinet Doors

Peninsula Hardwoods

Penn Sylvan International

People Logic Software Corp.

Pinske Edge

Pioneer Lumber Company

Pioneer Millworks

Plogic Solutions Ltd.

Pond Cove Paint

Porter-Cable

Precision Drive Systems

Premium Specialty Hardwoods

Prime Estimating and Software Services, LLC

Primo Woodworking Machinery

Pro.Woodworker.com

Pro100

Professional Hardware & Supply Co.

Professional Machinery Group

PYTHA

Quality VAKuum Products, Inc.

Quick Machinery Company

Quickscrews International Corporation

QuickScribe

QuikDrawers

R&R Drummond, Inc.

R.A.W.

R.D. Billhofer Company

Rangate

Rawles-Aden Lumber Corp.

RazorGage

Rex Lumber Company

Riethmiller Lumber

Ritter Manufacturing Inc.

Rockler Woodworking and Hardware

Roger Shaw and Associates

Rose Machinery

Routech

RouterCAD




Troubleshooting Failure with an Iron-On Dried-Glue Veneer Application       Pros discuss the probable reasons for bubbling of veneer that was applied using a hot iron and dried yellow glue. September 27, 2008

Question
I used the dried yellow glue and ironing method to bond an expensive maple burl to a small table top. Finished it with three coats of homemade oil/varnish and then two coats of water based polyurethane (Minwax). Now there are several bubbles randomly scattered where the veneer is apparently delaminating! Do you think I can rebond it with more heat and pressure from an iron or am I doomed to start over?

Forum Responses
(Veneer Forum)
From contributor J:
Burl and tensioned species are best laid up with a urea resin glue line due to its rigid properties. Other woodworkers have injected CA glue into such problem areas with varying degrees of success. It may re-bond with additional heat but I do not know how it would affect the finishes.



From contributor R:
Best bet is to start over. You'll find by the time you start cutting the veneer open and injecting glue and trying to re-stick it and on and on, you'll wind up with the same problems you started with. Try to find a shop in your area that has a press and have them do it. It may cost a little more but you'll save in the long run.


From contributor D:
The dry glue and hot iron method was touted by a leading woodworking publication and as such, has gained credibility by its mere publication. Why people just won't use veneer glues and proper methods, I don't know, but they insist on finding and using these odd and arcane methods that are totally unproven, especially over time. I'm speaking of the ironed glue and contact cement methods of veneering.


From contributor G:
If it was me, I'd be thinking about a syringe full of glue and a hollow needle. Will it work? Maybe. Will it fail down the road? You guess.

What is the substrate? How was it prepped? Is the veneer delaminating or is it lifting off the substrate? How thick is the veneer?


9/13 #8: HELP, veneer finishing problem ...

Jeff Jones
geppetto425@comcast.net

The ironing glue method is the same as ironing on pre-glued edging or glue-film veneer. Is it not PVA glue reactivated with heat? I am still a novice when it comes to veneer. I run a small one man shop and my veneer experience so far has been repairs and patching. This method appealed to me because it doesn't require special water-to-glue ratios, soaking time, temperature, or the other messes associated with hide glue. And by using an ordinary iron, there's no need for a vacuum bag, an expensive press or complicated clamping cauls. I also read that veneer applied this way does not cause any distortion. Because of the construction of this particular piece, I did not have access to the back side.

I used 1/4" hardwood plywood glued on the top for a flat substrate. After taping up the 1/64" veneer, I sealed it with a coat of 3-lb cut shellac (which is also thermoplastic like the glue). Then I applied two coats of Titebond III (note: waterproof), thinned 10% with water. When this was completely dry, I ironed it on with great results, it was very flat and secure. I lightly sanded the skid and light scorch marks off and waited several days before applying my homemade oil/varnish finish (1 part boiled linseed oil, 1 part varnish, 1 part mineral spirits). Three coats, rubbed in with 400 grit wet/dry. Okay, I should have stopped there. But I wanted a quick high gloss finish, so I started applying the water-based polyurethane... That's when the veneer started bubbling.

What is baffling me is why it has delaminated in several places even though the veneer was sealed with shellac and I used waterproof glue. Any chemists out there?



From John Van Brussel, forum technical advisor:
Edgebanding is usually pre-coated with an EVA hotmelt. PVA glues are an evaporative cure, which means they cure by giving off the water in the glue to form the bond. It is similar to latex paint. PVAs are thermoplastic, which means they are reactivated by heat. Think of this glue as being similar to candle wax; when it is cold, it is solid, and when heated, it will flow. PVA glues are also very high water content and consequently not the best glues for veneering, in my opinion. Another critical part of laminating veneer is to get uniform pressure over the entire surface. This is difficult to achieve using a hot iron and hand pressure except on smaller pieces like cigar boxes, jewelry boxes, etc.


From contributor R:
I've been making wood veneer panels for 18 years. In all these years I have been using catalyzed and non-catalyzed PVA glues with great success. The various glue companies have really formulated some excellent PVAs over the years. The urea formaldehyde glue is old school and works well, however it is not the healthiest stuff to be around. The powder and the fumes it gives off are not very lung friendly. The yellow glue, i.e. Titebond, is an aliphatic resin somewhat in between PVA and urea. PVAs and Titebond dry by the evaporation process, whereas ureas dry by a chemical reaction. Either way, once these glues fully cure, it is pretty much impossible to reactivate them.

I have used the dried yellow glue and iron method and have had a 50/50 success rate. There are many variables involved here when you try this method. Proper glue spread, the right time to start applying heat, how much time to keep the iron in any particular spot.

Did you scuff your substrate and make sure there was no debris or excessive dust, oil or other foreign matter that would cause the glue to fail? Was the veneer also inspected for the same things? This could be the reason for your problem. Was the caul board that you used perfectly flat? When it comes to veneer work, prepping of all your material prior to any glue-up is the most critical, because once you start spreading glue, there is no turning back.

Once again, think it through and go for it. Mistakes will happen, but that's part of the learning process. And to reiterate, it will probably be better to start over. In my experience, once the glue has dried and a finish has been applied, the work piece is pretty much impossible to repair and wind up with a quality product. Don't get me wrong, it is possible to fix, but by the time you fool around with it and possibly get it fixed, you could have re-done the piece with much better results.



From contributor P:
I think the bubbling is most likely from using waterbased poly over the veneer - this is like dumping water on the finished piece and will stress the glue lines. But at the heart of it is your method for applying the veneer. A handheld iron simply doesn't provide enough pressure to make a durable glue line. And to assert that applying a hot iron to wood doesn't stress it is absurd - whatever moisture is in the veneer is being forced out at the same time that the veneer is being locked into place, so it is quite likely that the addition of moisture in the future will cause bubbling. I also wonder about your application of a 1/4" substrate to the top of the table - was it originally a solid top? Even if it was veneered, you have now created an unbalanced panel, which will certainly cause problems down the road.

Stepping back a level, just because it's been printed doesn't mean it's a good idea. Fine Woodworking also printed an article called "Make a chair with biscuits!" or something like that, which is very foolish. Magazines need new content all the time, and will often print dubious advice in order to fill pages. Much of what they write is aimed at hobbyists, and makes no sense for professionals. Techniques which do no harm in a home hobbyist situation can be inappropriate and even dangerous for professional use.



From contributor C:
The likelihood of successfully veneering a large surface with a handheld iron and a thermoplastic adhesive is very low. That said, I have had great success using this method to apply edgebanding in certain circumstances.

You can make a low cost veneer press in your shop by constructing a torsion box and using bar clamps around the box's periphery to clamp the veneer down. Ian Kirby wrote an article on this in Fine Woodworking's earlier book titled "Marquetry and Veneer." I have never tried this method, yet if the torsion box is made properly, I have no reason to doubt it would work well.

On one occasion I had to inlay a strip into the center of the table. I placed the substrate on the floor and wedged 2 x 4 studs between the caul and an I-beam directly overhead. With a thick enough caul, or a torsion box, and of course a sturdy enough ceiling, you can do the same.

I (and people who work for me) will iron on veneer edges in the following circumstances:
1. A perfect continuous grain match between the top and the edge is necessary, and
2. The shape of the edge precludes any kind of clamping.

We experimented with aliphatic resins, PVAs, and UF (UniBond 800). The Unibond worked well, but was the nastiest application of an adhesive I have ever undertaken. It stunk and I know the fumes could not have been good for my health. The results, however, were fantastic. I used that method on an ebony desk with an avodire edge 10 years ago.

Overall, we've had the best luck using white glue. Apply the glue to the substrate and the veneer the day before. Just before ironing on the veneer, brush on a light coat of water and when using the iron, press as hard as you can, plus a little extra. I wouldn't attempt this on surfaces larger than an edgeband.

The table below was made in 1998. The edges were ironed on with white glue. The top was glued in a vacuum bag with UniBond 800. I showed the table at the Philadelphia Furniture Show. Ian Kirby (an accomplished and well respected furniture maker) stopped by the booth and admired the table until he found out the edges had been ironed on. He said the edges will surely delaminate. The table is in my office and is used every day. The edges look like they were glued on last week. They're fine.


Click here for higher quality, full size image



From contributor W:
I was recently faced with a similar repair job. Small "bubbles" on a table top that I thought were places where the glue had not adhered proved to be small puddles of glue instead. Long story short, after trying the hot iron method, I removed the veneer and started over.

A water-base finish over an oil-varnish mix can be problematic. If this is a necessary process for you, I highly recommend that you allow enough time for the varnish-oil film to completely cure, about two weeks or more, before applying a water-base film over it. Bob Flexner's book, "Understanding Wood Finishing" has excellent information regarding the compatibility of finishes of different kinds.



From the original questioner:
I stand corrected about edge banding not using PVA but rather EVA hotmelt.

Yes, I lightly scrubbed the substrate and back of veneer with 80 grit to get rid of any nubs. It was as smooth as a baby's behind.

Contributor W, you are correct, that was kind of screwy on my part. I had just read an article in the latest Woodsmith, no 163, about this. One coat of oil varnish for color and depth, then water based polyurethane for speed of drying in a dust-prone home workshop. I started rubbing in more than one coat, though, and I should have let it dry longer than a week. (I should have just quit there instead of getting impatient!)

Here are some pictures of the offending piece. I took it to the customer the other day and they are actually very pleased with it. I am going to rub it out so it is a bit smoother, only charge them for the materials, and I will check back with them in a year and if it is worse, I will redo it gratis.

Before...


Click here for higher quality, full size image

After. You can see the bubbles at the top of one of the pictures.


Click here for higher quality, full size image



From contributor O:
As for your particular veneering issue, it would be worth the time and cost to purchase and learn the use of a good vacuum bag system. They are not very expensive and would eliminate this type of problem. At the same time, you should begin experimenting with urea glues. The iron-on method, despite being regularly promoted by the FWW group, is not for long term construction. Take the time to learn how to do it the right way. This forum is a good place to ask or research how to veneer the right way, preferable before you get to the gluing stage of a project.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Veneer

  • KnowledgeBase: Veneer: Techniques




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article