I would like to retard moisture change of plywood. The plywood has Maple/Birch decorative veneer with softwood core.

Based on internet research (mainly Gene Wengert's past response on this forum), it seems I have two options: 1) Vapor resistant finish, and 2) Plastic wrap.

Below are my questions:

1. What exactly is a “good vapor resistant finish”? What chemical composition or brands do you recommend?

2. Is the “vapor resistant finish” the UV clear coat commonly used on prefinished plywood?

3. Should all plywood surfaces (including the four edges) be sprayed with this “vapor resistant finish”?

4. As for plastic wrap method, what is the minimum thickness and type of plastic?

5. Should the plastic wrap be in the form of stretch wrap or gusseted plastic pallet bag?

6. What is the proper way of wrapping plywood to minimize moisture change?

1/26/23       #2: Storage: how to retard moisture cha ...
Mark B

What is you end goal? Stabilized shipping of raw material? Storage? Finish coating?

1/26/23       #3: Storage: how to retard moisture cha ...
Jenny Member

My goal is to stabilize the plywood for shipping (from plywood mill to my warehouse, then to UV contractor) and for storage in my own warehouse.

I am located in a dry climate and the plywood is coming from a wetter climate.

1/28/23       #4: Storage: how to retard moisture cha ...
Karl E Brogger  Member

Website: http://www.sogncabinets.com

Say you put it in a Ziploc bag, no moisture loss from the humid mill, to your dry shop.

Whay happens when you open the bag, and cut parts?

I feel like you want acclimation, not isolation to your environment.

1/28/23       #5: Storage: how to retard moisture cha ...
Tom Gardiner

What are other plywood exporters doing? They have millions invested in product and will have done the homework to protect their product. No need to reinvent the wheel

1/28/23       #6: Storage: how to retard moisture cha ...
Mark B

The assumption is your trying to stabilize import material that is going haywire who knows.

Bottom line I would guess is the only viable option is to 3 wrap ths units (clean folded sheet below, one on top, and a boat-style shrink wrap band is the only cost effective option. Any type of coating protection is only viable if its part of the fibal product (cost)

1/29/23       #7: Storage: how to retard moisture cha ...
Jenny Member

Please see the map below for average RH and MC for interior woodwork in various parts of the US. I have also attached a chart that shows RH and corresponding MC.

My workshop is located in Southwestern United States. Target MC for local orders is 5%.

I don’t have much experience with plywood. My company specializes in glossy contemporary lacquered doors and particleboard carcass. Recently, I have customers who strongly prefer plywood carcass and hence I am pressured to offer plywood carcasses.

I don’t import plywood from abroad. The plywood I plan to buy are produced in the Pacific Northwest. The UV contractor is also located in the Pacific Northwest.

I usually have my UV contractor picks up the plywood directly from the mill. He has found out that plywood's MC is always at 9-11% when he inspects at the mill. Because of the huge difference between 11% and my target MC of 5%, I worry that the plywood would warp when they arrive at my climate.

Questions:
I have read from Gene Wengert’s post on another forum that “When softwood plywood is manufactured, it would be typical to find 4 to 5% MC, as the heat used to cure the adhesive in a press tends to drive off the moisture. “

1. Based on this info, can target MC of 5% be achieved if the plywood mill is willing to wrap the plywood with plastic?

2. I don’t know how quickly moisture change occurs. How soon does the plywood mill have to wrap up my plywood with plastic?

3. After my UV contractor in the Pacific Northwest finishes clearcoating the plywood, does he have to package my plywood with plastic in a low-humidity room with 25% RH? How soon does the UV contractor have to wrap up my plywood with plastic?

4. It is likely that the plywood mill doesn’t want to change any of its usual packaging procedure. In which case, how should I acclimate my plywood?

Tom- I wonder how plywood mills in Oregon and Washington manage to sell to Southwestern states such as Nevada and Arizona. Do you know if it is common practice for plywood mills to produce 4-6% MC plywood for the southwestern market?

Mark- Thank you for suggesting the 3 wrap method. The plywood mills I am considering are located in Oregon and Washington.


View higher quality, full size image (640 X 599)

1/29/23       #8: Storage: how to retard moisture cha ...
Jenny Member

Thank you for your reply, Karl. Your response has given me a lot of think about.

My company specializes in glossy finish. I only sell assembled cabinets.

My customer base is people/businesses in skyscrapers in LA, Las Vegas, Phoenix and Miami. The plywood mill I plan to buy from usually produces plywood at 9-11% MC.

I plan to take the plywood out of the plastic bags only when I need to cut the components. The components will be cut by CNC in my shop’s general area (which has the local dry humidity of around 25% RH).

I have not decided if I should go for isolation or acclimation.

If the plywood mill wraps up the plywood when the MC is still at 5-6%, then maybe isolation is the better idea?

If the plywood mill only sells their usual 9-11% MC plywood, then acclimation is my only choice.

I have given this a lot of thought and I don’t know if I am getting paranoid. I may have been overthinking.

Now I have even more questions in my head:

1. Since I have customers in humid Florida (target MC of 11%), should the UV contractor in Oregon wrap plywood for Florida in plastic, so that plywood’s MC won’t decrease rapidly when it gets to my dry shop?

2. For storing cabinets going to Florida, should I humidify a closed-off room in my shop that matches Florida’s target MC of 11% (i.e. 58-63% RH), and have packaging occur inside this special room?

3. Is packaging in a special humid room necessary, or is packaging in shop’s general area good enough?

1/30/23       #9: Storage: how to retard moisture cha ...
RichC

Buy the shrink wrap they use to store boats over the winter. Wrap and shrink with a propane torch.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Limtech Industries, Inc. Lamello
    Today's Sponsors
    • Denray Machine
      Quality Dust Filtration Systems Provided by an Industry Leader in Wood, Metal, and Many Other Dust Control Applications
    • Safety Speed Manufacturing
      Economical Vertical Panel Saws, Panel Routers, Edgebanders and Widebelt Sanders
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Mereen-Johnson Machine Company
      Manufacturers of High Production Woodworking Machinery
    • WOODWEB, Inc.
      The Information Resource for the Woodworking Industries
    • Onsrud Cutter
      Router Tooling for Woodworking, Plastic and Non-Ferrous Metal Manufacturers
    • JKL Machinery
      US Exclusive Importer Casadei, Busellato, Vitap, Bonacin - Machinery Dealer representing New & Used Woodworking Machinery
    • iBiDMachinery
      The Nation's #1 Used Woodworking Marketplace - Buy and Sell Woodworking Equipment with iBiD!
    • OMEC/Macoser Inc
      Exclusive Importer of European Woodworking Machinery Since 1988
    • Country Saw and Knife
      Complete Sharpening Services for Wood and Metal Saw Blades, Jointer Knives, and Bandsaw Blades
    • Parts Cutter CNC
      CNC Cabinetry and Closet Parts
    • T-Tool USA LLC
      Quality Tool-Holders, Tooling Supplies and Accessories for Numerous Cutting and Grinding Applications
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!