Bubbles in cured waterborne finish

4/27/25       
Jim Member

I take on one or two commissioned projects a year for cabinet or furniture work. I struggle to get professional finish results, which is driving me crazy. Bubbles have been my enemy. My finish choices have been General Finishes (Enduro Var or White Poly) or Target (EM6000 or EM8000) water based finishes.

I critiqued my setup from top to bottom this year to weed out potential issues.

I installed new hoses and filters after the compressor in addition to a Whirlwind filter at the base of the guns.

The shop is warmed to 70 – 75 degrees F. with the finish at a similar temperature. Humidity is 50 – 60%. I stir and strain the finish through a medium mesh filter the night before into PPS cups to allow some time for bubbles to settle out.

I generally build with maple, cherry, or walnut. The surfaces are sanded to 220 grit. Dust is removed with a blast of filtered air and/or a microfiber cloth (no tack rag.) I may apply a one pound cut of dewaxed shellac to highlight the grain, which I mix up in house. I allow it to cure for a day or two before the top coats are applied.

With a Devilbiss FLG4 gravity HVLP gun, pressure is set to 18 psi with the trigger pulled. On a Sata knock-off RP gravity gun, I have the pressure set to 28 psi. I aim for 3 mil wet film thickness, sprayed about 8” away with 50% overlap.

I have adjusted air pressure, film thickness, spray distance, room and finish temperature, viscosity, retarder, fan on/off, 1.3 or 1.5 mm tip, etc. A couple minutes after spraying, bubbles are everywhere. I come back 30 minutes later hoping they would settle out, but it just isn’t a quality result. The first coat or two are fine as the wood absorbs, but once the surface is sealed, bubbles are very evident after curing; in a quartering light they are visible and when you run your hand across the surface it is not as smooth as it should be. The spray guns are cleaned after each session with warm water, followed by watered down denatured alcohol.

Target and General Finishes haven’t given me satisfaction, and I have combed through Woodweb and other blogs. I would greatly appreciate any ideas!

Jim

4/28/25       #2: Bubbles in cured waterborne finish ...
Leo G Member

Sounds like you've gone through the gamut. As I recall Target wants 2-3 mil per wet coat. It's pretty light. Not to hard to go overboard. Make sure there is minimal or no airflow over your parts while they dry. Same thing with heat sources. Nothing direct on the parts until they've flashed.

I would stay away from the shellac, but I understand you wanting the glimmer from the shellac vs the pretty dead waterborne finish.

Are you scuffing with their recommended type of sandpaper? Not grit, sometimes they want no stearates in the paper or a certain abrasive medium.

Good luck.

4/28/25       #3: Bubbles in cured waterborne finish ...
Bart

Long time 20+yr GF user here. And full time cabinet finisher/long time woodworker.

Our setup is roughly the same I've got multiple flg-4's I use for stain, shellac(under pigmented GF), pigments and clears. But I use a 2.2 tip in all of them. And I run them at 45-65lbs at the compressor on a 50ft hose with no gauge at the gun. I adjust by feel not lbs of air. And I only have water trap at the compressor.

I've used Zinnser dewaxed many times and a couple of times a 1lb cut from chips I mixed in house under GF w/no issues. And all my GF pigmented work has Zinnser shellac primer under it to keep the grain raise at bay.
Key is 1st coat of GF sealer needs to light. Light sand and off to the races w/1-2 coats of SS and then topcoats. Have used the Endurovar once on some floors with no issues.

One key I've found w/WB is moving plenty of air over them as they dry in the racks. Flashes them off quickly. And no issues ever w/bubbles. I never turn the fans off until all pieces have flashed off. That could something to look into.

Also I would never use micro fiber, too much bite. I use a well broken in cut up cotton t-shirts/rag mostly for the dustiest pigmented/undercoat stuff. I think the current one is running on a few years old. But mainly parts are aired off and good to go.

I use warm water clean up as well. I'll run 2-3 cups through the gun after a session. I would stay away from any solvent unless your doing a thorough cleaning and then I would want to shoot a couple of coats of sealers before any topcoats to clear any debris/solvent that might linger.

I don't think 220 is necessary. Especially on hardwoods like maple, oak or walnut where burnishing can be an issue. I only go to 150.

BTW have you shot some finish on a clean piece of glass? If it's a contamination issue it will show up there.

my2cts
cheers Bart

4/29/25       #4: Bubbles in cured waterborne finish ...
Jim Member

Thanks Leo and Bart. I have some homework to do with your feedback, starting with shooting on glass, trying a larger fluid tip, and managing air flow.

I have been doing woodworking projects for 40 years. So many of the "fine furniture" folks are leaning toward wax/oil products such as Osmo and Rubio, and they have their place. But an off the gun, smooth as silk finish can really make a statement as well. I started with a Fuji turbine for a kitchen project 10 years ago and it worked fine. As I migrated to a compressor based setup, I was hoping the increased flexibility would give me more consistent results as I dial in the sweet spot. But there are days where it feels like the choke is stuck open and things just don't come together for all the prep work.

4/29/25       #5: Bubbles in cured waterborne finish ...
Leo G Member

Finishing is 1 part chemistry and 3 parts voodoo.

4/30/25       #6: Bubbles in cured waterborne finish ...
Fred Melton

Not an expert on water base finish I do know after spraying cv for over 25 years if a finish is making bubbles in finish you need to restard slow done drying so air will seep out of the wood ,a sealer coat can help it penetrates down in your wood

5/4/25       #7: Bubbles in cured waterborne finish ...
Jim Member

In the last few days I experimented with

a. 1.3, 1.5, and 1.8 mm nozzles
b. tack off with a lint free rag
c. drying with and without air moving
d. spraying glass
e. 15 psi, 18 psi, and 22 psi at the gun with the trigger pulled

The attached picture shows the bubbles a couple minutes after spraying on glass. I didn't see any obvious contamination.

The above iterations didn't give me solid results. At 15 psi overspray was minimal, but the end result was still too many bubbles dried into the finish.

My gut says lower air pressure, increased spray distance, thin coats, and added retarder would be the better of the tweaks, but I can't land a quality finish. If 95% of the bubbles dissipate during curing, the remaining 5% is too many, and it is time to try a different finish.

Bart with your experience with GF, what do you recommend for clear topcoat for casework and furniture?

Thanks!


View higher quality, full size image (4000 X 3000)

5/4/25       #8: Bubbles in cured waterborne finish ...
Adam C

I've been using the GF enduro, for a few years, now, for the most part I don't get bubbles, I am not sure why you are getting them, I spray the clean with a 1.8 cheap gun from amazon, I use the sanding sealer I find that works better at sealing in the wood. the finish is not slick to the touch like lacquer but I don't get air bubbles with it drys, I mostly use the 2k

5/5/25       #9: Bubbles in cured waterborne finish ...
Bart

How old is the finish ur shooting? It's also possible you got a bad batch, GF has a Mfg date just above the barcode. Apprx 10yrs ago I had back to back to back problems w/fisheyes. Pulling my hair out. Cleaning EVERYTHING. Worked w/local GF rep. Turns out all 3 gallons were from the same batch. New batch. Problems gone.

For clears/stain & clear. I use 2 coats S Sealer and 2 topcoats of flat poly.
And I like wet coats. I usually warm the finish in bucket of hotish water or set them in the sun well before use. On the sealer I'm at 3.5-4 turns out on the FLG and 2-2.5 turns out with 10% thinned/warmed flat poly topcoat. I can't imagine using anything less than a 2.2 tip. My arm would fall off. :)

On my pressure rig it's the same only with a 1.1tip. Blow and go.

If it's a furniture piece with no water/wear issues I like 3 coats for a tighter nitro look. Also I add a dash of orange dye to give it a solvent sorta look. WB can look a little plastic-y. Or shoot some dewaxxed shellac under it. Boom.
I did a whole set of kitchen uppers with $$$$ curly maple veneered slab doors/panels w/dewaxxed and GF over it. It was incredible.

For added smooth sometimes I'll hit panels and doors with well used 2000grit. Just make sure you clean/wipe down including the sandpaper before one very light one pass. About as good as you can get off the gun.

BTW, I have two box 24" fans on high going over my drying racks. It ain't subtle. Especially good for vertical surfaces.

Hope things work out
Cheers
Bart

5/6/25       #10: Bubbles in cured waterborne finish ...
Jim Member

Thanks Bart and Adam.

I have not ruled out a bad can of finish. I have had it for a couple months in a conditioned space. I am very familiar with the feeling of pulling my hair ….

My finish schedule is similar to yours Bart. I will add a hint of color at times through dewaxed shellac or Transtint. I back the needle out about 3 turns for a 1.3mm nozzle, with 10% reduced or finish warmed to about 80F, depending on what mood I’m in. You spray with a little larger nozzle, which I will experiment with in the future and choke the needle back a little.

I love unadulterated maple. I did my own kitchen in a 5 piece door using curly as the panel. The world has gone for white and gray cabinets, but I do like the simple richness of maple. I have used white scotchbrite or craft paper to knock down the over spray "roughness." I’ll sample 2000 grit in the future.

I’m gonna order a can of Enduro ClearPoly to run some test panels next week. I appreciate your time.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!