Choosing panel material for counter doors

6/11/23       
Andrew

Hi, I am looking for some advice .

The project is a millwork counter for a commercial cafeteria (solid surface top if it makes a difference to your answer). The base is 3/4" water resistant Douglas fir plywood (DFP) construction finished with plastic laminate (P.Lam). The spec calls for doors to also be 3/4" DFP but with hardwood trim on all edges, and matching P.Lam finish.

I have been asked to consider MDF with hardwood trim and P.Lam for the doors only. The proposal argues that the MDF is less likely to warp compared to DFP. While I agree with the logic, I am concerned (being a high traffic, potentially high moisture environment) that MDF may swell.

I have seen warped DFP doors and particle board that has disintegrated if the P.Lam is compromised even slightly, but have no experience with MDF cores. Other than potential warpage, exterior grade DFP seems like the best choice based on my research.

What are your thoughts/recommendations? Do you have a preference? Are there other options that should be considered?

Thank you.

6/11/23       #2: Choosing panel material for counter ...
Leo G Member

MEDEX water resistant MDF. I use it in kitchens for painted panel material.

6/12/23       #3: Choosing panel material for counter ...
Andrew

Thanks @Leo G, I appreciate the response. I will look into Medex.

Are there any special treatments to improve screw hold or is that not an issue with Medex? (Again, working from hearsay not experience)

6/12/23       #4: Choosing panel material for counter ...
Leo G Member

If you are screwing into the face, as long as you don't over tighten and strip the threads in the wood it'll last a good long time.

If you are screwing into the edge it'll work better than regular MDF but not by much. Edge screws into most engineered products isn't that good and that included plywood because it can split on the glue line.

6/20/23       #5: Choosing panel material for counter ...
Bruce H

You can buy MDF that is water proof. I have some that has been in a jar of water for a year without change. Wouldn't have believed it. I used it for window sills and porch columns. The stuff is made in the US from rice.

That said I did a coffee shop using mahogany marine grade plywood with laminate on two faces, 3mm edge band. It was the nicest stuff I have ever used, expensive though. You couldn't run fast enough for me to try this on Douglas Fir plywood.

8/18/23       #6: Choosing panel material for counter ...
Laura Member

Choosing the right materials for a millwork counter in a commercial cafeteria is crucial to ensure durability and longevity, especially in a high traffic and potentially high moisture environment. Both DFP (Douglas fir plywood) and MDF (medium-density fiberboard) have their pros and cons, so let's break down the considerations for each:

DFP (Douglas Fir Plywood):
Pros:

Water-resistant properties, especially when sealed and finished properly.
More structurally stable than MDF due to its layered construction.
Generally more impact-resistant than MDF.
Better screw-holding capabilities.
Familiarity in working with plywood for construction.
Cons:

Can warp if exposed to significant moisture or not sealed properly.
Heavier than MDF, which could affect ease of installation.
Variability in quality, depending on the grade and manufacturer.
MDF (Medium-Density Fiberboard):
Pros:

Less likely to warp compared to solid wood or plywood due to its uniform composition.
Smoother surface, which can be advantageous when applying laminate.
Easier to shape and cut intricate designs if necessary.
Generally more affordable than higher-grade plywood.
Cons:

Prone to swelling and disintegration when exposed to moisture, especially if the laminate is compromised.
Not as impact-resistant as plywood.
Heavier than particleboard but lighter than plywood.
Given your concerns about moisture and the potential for swelling with MDF, it's understandable to hesitate in using it for a high-traffic, potentially moisture-prone environment like a cafeteria. While MDF is less likely to warp compared to solid wood, its susceptibility to moisture-related issues could be a significant drawback in your situation.

Based on your description, exterior-grade Douglas fir plywood with a hardwood trim and plastic laminate finish seems like a prudent choice. It combines the water-resistant properties of plywood with the added durability of hardwood trim. Proper sealing and finishing techniques will be crucial to prevent warping and moisture-related problems. Regular maintenance and quick action in case of any laminate damage will also help prolong the life of the counter.

10/27/23       #7: Choosing panel material for counter ...
David William  Member

Website: http://www.bergenfurniturenj.com/

For a high-traffic, potentially high-moisture environment, using exterior grade Douglas fir plywood (DFP) with a matching plastic laminate (P.Lam) finish for doors seems like a sound choice. While MDF can be a good option for some applications, it may not hold up well in areas where moisture is a concern. Given your concerns about potential warpage and swelling in such an environment, sticking with exterior grade DFP would be a safer and more reliable choice for the doors. Additionally, proper sealing and maintenance of the P.Lam can help ensure longevity and durability.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors

    Become a Sponsor today!