Today's
Sponsors:


BetterVacuumcups.com

Biesse America

Biewer Lumber

Binks

Black Bros. Co.

Blackhawk Machinery

Briquetting Solutions by Sunomi LLC

Brown Wood Products Co.

Business Management Solutions

Byrd Tool

C.R. Onsrud

Cab Parts

Cabinet Door Service Co.

Cabinet Pro

CabinetCRUNCHER Cutlist & 3D Cabinet Design Software

Cabinetmakers Association

CADCABINETS.COM

CADCode

Cag Lumber

Cantek America

Carolina Woodworking Consultants

Carter Products

Carving Technologies

Castle

Catskill Timber Industries

Charles G.G. Schmidt Co.

Chicago Dowel Company, Inc.

Clear Lake Lumber

CNC Parts Dept.

1-800-Cabinets.com

2Sand.com

3M Corporation

A O M Spray Equipment

Abrasive Resource

Accu-Router, Inc.

AceCo Precision Wood Tooling

Activa

Air Handling Systems

Alan McIlvain Company

Algoma Lumber Co.

All Star Adhesives

Alliance Millsoft

Allied Machinery Inc.

AllRout

Amana Tool

Ameitech South

American Fabric Filter Co.

American Institute of Building Design

American National Woodworking Knife

American Rotary Converters

Andreou Machinery

ANEST IWATA USA, Inc.

Antique Beams and Boards

Antique Building Materials

Anver Corporation

Apollo Sprayers Inc.

Arbor Processing Inc.

Architectural Elements

ArtCam

ATEMAG

Atlantic Machinery Corp.

Auton Motorized Systems

AWFS

B.H. Davis Company

Bailey's Inc.

Baker Products

Banks Hardwoods

Barn Detail

Barn Door Lumber

BC Wood Specialties Group

BeamsRUS

Beaver Tools

Benz Incorporated

Best Cabinets




Mixing African and Honduras Mahogany       A long discussion of the woodworking characteristics of various Mahogany types and substitutes, and the practicality of combining different woods in a single door. June 29, 2008

Question
We are a small shop and make solid mahogany exterior doors with 2-1/2" long mortise and tenon joinery, epoxied and pegged through. Availability, quality and price are dictating that we make the transition from Honduras (pattern grade) to African (Khaya, straight-grained, FEQ/pattern grade - no ribbon). What I've seen of it looks indistinguishable from Honduras.

What are the implications of mixing the two in one door? They are so close in specs for shrinkage, if we select for similar grain and density, would it matter? Is it ok for paint-grade? Ok/not ok for stain grade? Do we need to try and keep the inventory separate or can we mix them thru the transition? My number one concern is/has always been quality and structural integrity and I don't want to sacrifice either.

Forum Responses
(Architectural Woodworking Forum)
From contributor P:
I frequently mix both species, but I do so carefully. Examples like making the stiles and rails from Hondo and the panels from African. I can tell the difference between the two for most cuts, so I mix and match accordingly.

I still prefer Hondo, but as the quality and supply diminishes, African is a fine substitute. I have a few thousand BF of FEQ Hondo left, so I use it wisely, often making laminates to stretch my supply.

African seems to behave fine in service, I do not like the bigger pores and I find it had much more internal stress than Hondo. That may not be the species, but the drying. Just be sure to be honest with your customer and tell them exactly what it is you are using.



From contributor A:
I think it is fine to mix Hondu and African. Paintgrade and staingrade are no-brainers. Clear coats might give it away. It's really based on a side by side comparison. I've had some saepelle that looked identical to pattern Hondu in a side by side. Why are you still pegging while using epoxy?


From Gene Wengert, forum technical advisor:
You might also look at sapele (pronounced sa-pee-lee), which is often used as a substitute and is in the African mahogany family.


From the original questioner:
Thanks for the feedback. We epoxy and peg because it locks the joints without clamping and it adds to the beauty and character to see the dark end grain of the pegs against the face grain. I don't worry about joints failing.

Dr. Wengert you've got me a little befuddled. I've researched your comments on mahogany and you have said that sapele and Santos are unrelated mahogany and because they look similar to mahogany have been called such by lumber sellers doing creative marketing. You said that sapele is being called African by some lumber sellers, but that there is no genetic relationship and that sapele is not African mahogany and not a real mahogany at all.

I've been researching the alternatives for some time and have compared, at least on paper, Hondu, African (Khaya), Spanish cedar and sapele. African was the closest in spec to Hondu in stability, which I've always considered the most critical characteristic for an exterior door, especially tall ones, and we build a lot of those. sapele came in last in the specs for stability. African looks the most like Hondu, so I've read, from various sources. From what I've seen so far (and I haven't seen lots of it), that's been true, though I understand there are definite variations in grades (as there are in Hondu). I've not seen sapele or Spanish cedar.

Why African? We have been using Honduras mahogany exclusively for many years. It has been a key component of our marketing and we have return customers who already have our doors. FEQ grade African seems to be the choice that would be the closest in quality, stability, appearance, color and name.

Dr. Wengert, what is your opinion about mixing the two in a single door? If the parts had similar grain and density, do you think it would be problematic?



From Gene Wengert, forum technical advisor:
I would not support the idea of mixing species in the same door. I have seen a lot of exterior sapele doors.


From Gene Wengert, forum technical advisor:
The following appeared in FDM magazine (copyright by FDM 2006)
SAPELE
Gene Wengert
Sapele (pronounced sa-pee-lee) is in the African mahogany family. Indeed, sapele (Entandrophragma cylindricum) has the appearance of African mahogany; that is, sapele is dark reddish brown with a ribbon pattern. It is actually heavier, stronger and harder than mahogany. Its excellent working properties and wonderful appearance result in a moderate to high price in the lumber market. This wood is also available as veneer.
The tree grows in the tropical rain forests of eastern Africa, ranging from the Ivory Coast to the Cameroons and eastward through Zaire to Uganda. On the edge of its range, it has been harvested heavily and may be nearing extinction; however, it most of its range it is more plentiful and can be grown in plantations, assuring good supplies into the future with good forestry practices.

The tree in the natural forest will reach a height ranging from 100 to 150 feet, with some trees reaching 200 feet in height Tree diameters can reach 6 feet, although 4 to 5 feet are more common.. The merchantable stem is typically straight, free of branches and over 100 feet long. As might be imagined, this large tree produces tremendous volumes of clear lumber and veneer.

As the tree is growing, the vertical cells do not align vertically in the tree, but are aligned at a small angle. In other words, the grain spirals up the tree, similar to the stripes of a candy-cane. The direction of rotation also reverses from year to year. This phenomenon is called, when the wood is sawn into lumber, interlocked grain. When quartersawn or riftsawn, this interlocked grain creates a wonderful (and desirable) ribbon pattern on the face of the lumber.

As with many imported species, this wood is subject to attack by powderpost beetles. They can be eliminated by fumigation or subsequent, prompt kiln drying.

PROCESSING SUGGESTIONS AND CHARACTERISTICS
Density
Sapele is similar in density to red oak, but heavier than mahogany. Kiln-dried wood has a density of 36 pounds per cubic foot. Lumber planed to 3/4" thickness 7% MC will weigh about 2-1/4 pounds per board foot.

Drying
Sapele may be dried at the sawmill, but it is not uncommon to bring the wet wood to the USA for drying. It dries rapidly, but the interlocked grain results in a strong tendency to warp. This warp is best controlled by excellent stacking and low initial temperatures. Kiln schedules are similar to red oak. Overall shrinkage in drying (about 5-1/2% in width of flatsawn lumber and 3-1/2% for quartersawn) is not excessive.

Gluing and Machining
Gluing is moderately easy, but with the high density of the wood surfaces should be flat and freshly prepared. There are no resins to deal with. The interlocked grain means that on quartersawn and rift surfaces, the tool is always cutting some of the fibers "against the grain." Tear-out (torn grain, chip-out) is therefore likely, especially for low MCs and slender knives. The hook angle should be small so that the knife acts more like a plow than like a splitting chisel.

Stability
This wood moves somewhat in service when the humidity changes. Quartersawn lumber that shows the ribbon stripe will actually be fairly stable in width, requiring a 6% MC change to produce a 1% size change. Flatsawn lumber will move 1% with a 4% MC change.

Strength
Sapele is a little stronger than red oak. The bending strength (MOR) is 15,300 psi, the elasticity (MOE) is 1.82 million psi, and the hardness is 1510 pounds. Screw and nail holding is very high; predrilling of screw and nail holes near the ends of the pieces may be suggested to avoid splitting.

Color and Grain
Sapele is almost always 100% heartwood. The heartwood is dark reddish brown with a purplish cast. The grain texture is rather fine, similar to mahogany. The interlocked grain on quartersawn surfaces produces the ribbon like pattern. There is a very slight aroma at times which smells a bit like cedar. When sanded smooth the wood has a slight luster. It may be necessary to use a sealer on the wood surfaces (or use multiple coats), as there can be variations in absorption of the finishes without a sealer.



From Gene Wengert, forum technical advisor:
Anytime that wood warps immediately when machining, it is due to drying stress (which should have been removed in the kiln) or growth stress. Warp that occurs 5 minutes, 5 hours, 5 months, etc. later is due to moisture change and the resulting shrinkage or swelling.


From contributor P:
I use khaya and sapele on a regular basis and seldom have trouble with it. Personally, I love both of them.


From contributor A:
I did a complete bathroom in sapele and loved it. I thought it was going to chip like crazy when I saw all of the ribbon stripe. But I really didn't get any chipping of any kind. A lot of the sticks could run through the jointer in either direction with no tearout.

This is the exact opposite of my experience with the other African's. They also tend to have ribbon stripe, but tear out like crazy. The last time I had to buy some 8/4 African I paid my dist to sort the ribbon out of my delivery. I like the sapele better than most of the pattern SA I 've bought in the last five years.



From the original questioner:
With what I'd read about the interlocking grain of African and sapele, tear out was a definite concern, so it's interesting to hear your input Contributor A.

As far as mixing species in one door, my worry is that it could happen unintentionally, by mixing our inventory, especially shorter rail and panel stock that accumulates over time. Unless the guys doing the dimensioning are vigilant about marking every cutoff and keeping them apart, I'm worried they'll get mixed and I won't even know it, if it looks the same. Any tips on a good system for managing the inventory, especially in a smaller shop where real estate is limited? I was thinking maybe color coding?



From contributor K:
It doesn't tear out too bad, and a little water helps when it does. It will get fuzzy on the alternate strip though. You do have to watch the ends because little pieces will blow out, but as long as you allowed for this, it's not a problem.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Cabinetmaking

  • KnowledgeBase: Cabinetmaking: Cabinet Door Construction

  • KnowledgeBase: Lumber and Plywood

  • KnowledgeBase: Lumber & Plywood: Wood Identification




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article