Today's
Sponsors:


BetterVacuumcups.com

Biesse America

Biewer Lumber

Binks

Black Bros. Co.

Blackhawk Machinery

Briquetting Solutions by Sunomi LLC

Brown Wood Products Co.

Business Management Solutions

Byrd Tool

C.R. Onsrud

Cab Parts

Cabinet Door Service Co.

Cabinet Pro

CabinetCRUNCHER Cutlist & 3D Cabinet Design Software

Cabinetmakers Association

CADCABINETS.COM

CADCode

Cag Lumber

Cantek America

Carolina Woodworking Consultants

Carter Products

Carving Technologies

Castle

Catskill Timber Industries

Charles G.G. Schmidt Co.

Chicago Dowel Company, Inc.

Clear Lake Lumber

CNC Parts Dept.

1-800-Cabinets.com

2Sand.com

3M Corporation

A O M Spray Equipment

Abrasive Resource

Accu-Router, Inc.

AceCo Precision Wood Tooling

Activa

Air Handling Systems

Alan McIlvain Company

Algoma Lumber Co.

All Star Adhesives

Alliance Millsoft

Allied Machinery Inc.

AllRout

Amana Tool

Ameitech South

American Fabric Filter Co.

American Institute of Building Design

American National Woodworking Knife

American Rotary Converters

Andreou Machinery

ANEST IWATA USA, Inc.

Antique Beams and Boards

Antique Building Materials

Anver Corporation

Apollo Sprayers Inc.

Arbor Processing Inc.

Architectural Elements

ArtCam

ATEMAG

Atlantic Machinery Corp.

Auton Motorized Systems

AWFS

B.H. Davis Company

Bailey's Inc.

Baker Products

Banks Hardwoods

Barn Detail

Barn Door Lumber

BC Wood Specialties Group

BeamsRUS

Beaver Tools

Benz Incorporated

Best Cabinets




Squaring Up a Cross-Cut Sled       Getting a cross-cut table-saw sled jig squared up just right is a finicky and time-consuming process. June 30, 2007

Question
I'm having trouble squaring up my newly constructed crosscut sled. I've got 1 1/2" thick front and back fences fastened to a 24 x 30" 1/2" MDF base. The front fence is attached with hex bolts allowing for slight adjustments. Table saw blade appears to be perfectly perpendicular to front fence. (I'm using a 12" Starett square to check alignments.) Blade is also perpendicular with the MDF base of the sled. End cuts on medium-sized boards appear perfectly square. If I take a 12" x 12" piece of 1/2" ply, however, and cut each side in sequence (I just rotate the cut around adjacent sides), side #4 is not a perfect 90 degrees with side #1. It's off by about 3/64's. I have tried adjusting the front fence slightly but nothing seems to work. Seems to me that if the blade, fence and sled base are all a perfect 90 degrees, then all cuts should be perfect 90 degree cuts. Any ideas? What could I be doing wrong?

Forum Responses
(Solid Wood Machining Forum)
From contributor J:
One possibility is if your blade is not very sharp, it could actually move the piece slightly as it passes through. Should be easy enough to check if you can mount a toggle clamp or some sort of stop to keep the piece from being able to slide.



From contributor O:
It seems like you're splitting hairs. You might be off 1/64" on your first cut, which might be hard to see. As you make your cuts, it just gets worse so on the third cut, you come up with 3/64". Try cutting in a different orientation and see what happens. If you're off 1/64", that's not much. It's not perfect, but maybe you could live with it. What type of runners are you using - steel or wood - and are they adjustable for your miter slots? Just a little bit of play can throw you off. If they are the adjustable type, you might be able to tweak them a little to true it up.


From contributor G:
Tweaking jigs is always time consuming. On a cross-cut sled, I wouldn't accept 1/64" of an inch per cut. You will never succeed in adjusting by trying to test with a square, regardless of how accurate your square is or how careful you are.

To test your jig you need to start with a test piece of ply that has two parallel sides. Make sure that you start with a piece that is straight and parallel. Now using your jig, cut off a piece of your wood, flip end for end and cut a 1" wide strip. Use a caliper to measure the width of the strip you just cut. Adjust your cut so that there is no more than .002" difference between the thick and thin ends of your strip. Less is better.

Let's say you have made your cuts on the right side of your test board... The slice for testing always falls to the right of the blade. Now you must test your jig with cuts that always fall to the left of the blade. If you cannot get the left and right cuts to come out the same, it's because your jig is not straight (or the jig shifts in the table slots when you're pushing from one side versus the other). This is a common problem because the jig is usually weaker where the saw kerf goes through... and jig gets bent. Or the jig is straight overall, but the wood isn't dead flat, and the squareness depends on how long a board you are cutting.

Finally, if there is any play in between your slots and the runners for the jig, you will not get consistently square cuts. Also, if your fence is not perfectly rigid, you'll have problems. Ditto if the fence is not exactly right angles to the base of the sled.

By the way, if your hex bolt is 24" from the saw blade, pivoting the crosscut fence .006" will change your cut by .003" over the 12" test piece. These are rather small adjustments, and sometimes wood gets compressed and forms grooves and doesn't want to be nudged such a tiny distance. Also, four cuts, each off by .002", adds up to .008" off, which is probably acceptable, but less is better. When you are working in thousandths of an inch, even cast iron seems like rubber putty, but just keep tweaking it and you'll get it.

And while you're at it, measure the kerf that your blade makes by cutting a groove using your jig. Compare this groove with the one you get from using the saw arm. Any difference between these measurements and the saw blade width, and you can tell if your jig is indeed running parallel to the blade, or is wobbling, etc.



From contributor B:
Another item to check, just so you know you are not assuming anything, is that the blade is parallel to the slots in the table where your sled runs in. If they are not, you should align them. Make sure the saw is in tune before adding things to the equation.


From contributor L:
Go ahead and make the 5th cut and then check. We use a slider and the ply never comes square from the factory.

Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Panel Processing

  • KnowledgeBase: Panel Processing: Machine Setup and Maintenance

  • KnowledgeBase: Solid Wood Machining

  • KnowledgeBase: Solid Wood Machining: Setup and Maintenance




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article