Question
I build props for event decorating/rental and a while back I built 4 cedar harvest tables, on the fly, measuring 43" x 104". The top construction is 9 board biscuit joinery (alternating grain) - 1" thickness. Because of the urgency I didn't attach my aprons to the table top until the day of the event and the next day they were disassembled, transported and stored - separate tops, legs and aprons. Within 2 weeks I caught sight of the tops belly dancing into s-curves and cupped edges (as in the image below) at the tables ends, while the long outside edges remained pretty much true.

I know that had I properly joined the top to the apron immediately, and maybe added breadboard ends, I might have avoided this result. Similarly, gluing, clamping and screwing doesn't feel like it's going to be enough persuasion at this time, especially on the tops with the cupping on the corner edges (like the image below).

I've experimented with cedar steam bending - it's nice and I like it, but I'm apprehensive to try to build something big enough to house one of these tops if my chances of success are limited. What do you steam savvy carpenters think? Or how best to approach repair without steam and without widdling my big tables into consoles?


Forum Responses
(Furniture Making Forum)
From contributor H:
Was the bottom side of this top finished equally to the top? To me it doesn’t look like it because it absorbed more moisture than the top and expanded causing the curve upward. Screwing it down will only serve to make the top crack.



From contributor L:
The last thing you want to do is introduce more moisture into the scene by steaming. You need to go the opposite way and try to dry the warped side. Take your tabletop and put the convex side towards the sun so that it will dry out the moisture and let the top flatten out. Check on the top every 15 minutes, you don't want it to got the other way. I suppose you could use heat lamps too, but the sun is free and much more even. Don't do all the tops at once, do one first and see the results, if they are what you are looking for then proceed with the rest.


From contributor G:
I did similar with a blanket chest top. I left it in my car for 14 daylight hours for delivery later. Well, even with breadboard ends I had a minipogada. I brought it home, took the top off and placed in my bathroom for a couple of days, and every once in a while I turned on the hot water, closed the door and basically steamed it. Thing calmed down nice enough and it dried in a couple of days to equilibrium. Then it was refinished and delivered.


From Gene Wengert, forum technical advisor:
Indeed, steaming is one way to go. But it is not 100% perfect. What happened was that the top of the table was exposed to a dry environment and it dried quickly and shrinkage forces were large and the piece cupped. The back side, which dried eventually, did not shrink as much because it dried slowly and could not overcome the rigidity of the drier and stronger top. (Wood gets stronger when dry.) The same effect can occur if you have a dry table top and expose it to humid conditions and there is an excellent coating on the top, so only the back side shrinks or swells.

You need to:
1. Assure in the future that the wood is at equilibrium with its environment, as it takes a MC change for wood to warp. Then use a vapor resistant coating so that any RH changes will not rapidly affect the wood moisture content.

2. At this point, you need to restore the piece to flatness. Adding water slowly will not do a great job. Rather, add moisture quickly to the cupped face (the top). This will flatten the table. Then slowly re-dry it to the correct MC, holding it flat. It will likely not be perfectly flat, so you may need a large drum sander.

3. Alternate plan. Rip it into several pieces, joint the new edges that are perpendicular to the face and re-glue. Then sand it smooth.

Note: There is so much cup that even if you had secured the edges to the skirt, I doubt that you could have held it flat.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Knowledge Base

  • KnowledgeBase: Furniture


    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2018 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    335 Bedell Road
    Montrose, PA 18801

    Contact WOODWEB











  • WOODWEB - the leading resource for professional woodworkers


      Home » Knowledge Base » Knowledge Base Article