Today's
Sponsors:


Royce Ayr Cutting Tools

RT Machine Co.

Safety Speed Cut

Sand-Rite Manufacturing

Sandman Products

Sawmill and Woodlot Magazine

Schultz Forming Products

SCM Group USA, Inc.

SCM Group

SCM

Sears Trostel Lumber Co.

Shade Dri

Shomaker Lumber Company

ShopBot

SII Dry Kilns

Silvaris

Simantech

Single Source Cabinet Supplies

SIS Machinery

SK-USA

SketchList

SlipCon USA, Inc.

SnapDragon Associates, LLC

SNX Technologies

South State Machinery

Southeast Tool, Inc.

Sovereign Machine, Inc.

North Pacific Lumber

Northstate Hardwoods

Northtech Machinery

NPO BARS

O'Shea Lumber Company

Old Mississippi Brick and Heart Pine Company

Omnitech Systems

Onsrud Cutter

Open the Door Products

Opti-Sand

Optisol for Project Scheduling

Original Saw Company

Osborne Wood Products

Paragon Enterprises

Patton Cabinet Doors

Peninsula Hardwoods

Penn Sylvan International

People Logic Software Corp.

Pinske Edge

Pioneer Lumber Company

Pioneer Millworks

Plogic Solutions Ltd.

Pond Cove Paint

Porter-Cable

Precision Drive Systems

Premium Specialty Hardwoods

Prime Estimating and Software Services, LLC

Primo Woodworking Machinery

Pro.Woodworker.com

Pro100

Professional Hardware & Supply Co.

Professional Machinery Group

PYTHA

Quality VAKuum Products, Inc.

Quick Machinery Company

Quickscrews International Corporation

QuickScribe

QuikDrawers

R&R Drummond, Inc.

R.A.W.

R.D. Billhofer Company

Rangate

Rawles-Aden Lumber Corp.

RazorGage

Rex Lumber Company

Riethmiller Lumber

Ritter Manufacturing Inc.

Rockler Woodworking and Hardware

Roger Shaw and Associates

Rose Machinery

Routech

RouterCAD




Veneer buckling       Preventing veneer from expanding and buckling through proper gluing and application methods. November 7, 2000

Q.
Why might veneer expand after 3 months of being finished and installed? In several places where the veneer comes together it seems as though it is pushing up at the seams. The contact glue used is the green from Wilsonart. I've had the finish checked with a dry mill gauge and it's okay. It is random, and occurs on mdf and ply, but mostly mdf.

Forum Responses
I have found out that when using contact cement a minimum of two coats on each surface is required. Let it dry between each coat. Then apply the veneer to the substrate. Iron on the veneer and then drag a veneer hammer or some other type of pressure device over the surface with as much pressure as possible.

I let it sit over night before trimming because it does grow or creep. In most cases that holds and it seems to be stable.

If that doesn't work use a resin glue on it, but that takes hours to dry. You need clamping or a vacuum system for that. I have also used yellow glue and ironed it on, but I find that creeps also. I did a 10 foot by 30 inch counter top for a credenza with mahogany veneer and I used the resin glue on that under vacuum. It looked like one large board when it was done.



Whenever you use contact cement with veneers there is a risk of delamination because of the finish solvents attacking the cement. I solved that problem for myself by buying a vacuum press. The glue I use with this is a Unibond 800 (207-725-0935), which is a two part Urea Formaldahyde. It takes a long time to cure but this would solve your problems in the future.


Contact was designed and invented for plastic laminate. It is flexible and designed to glue down a ridge product. When the woodworker took contact adhesive (a flexible glue line) and said let's lay sheet veneer, it all started.

Flexible sheet veneer was designed to be applied with a ridge glue line and a press. The manufacturers found out in a hurry that not enough woodworkers had a press or wanted a press. So the following instructions were agreed upon by most of the flexible sheet veneer manufacturers.

1. Both surfaces shall be free of all dust before applying contact.
2. Contact adhesive should be applied in a box coat method (applied in both directions).
3. 100% coverage applied to both surfaces (Approximately twice as much as required for plastic laminate).
4. Drying time is very important. Don't trap gases. It is the gases that cause the blister and surface checking. They are a natural process in contact, so it is up to you not to get the gases trapped. If you wait 15 extra minutes now you can save money later.
5. Maximum pressure should be applied by use of a wood scrapper. DO NOT USE A J-ROLLER ON SHEET VENEER. Applying maximum pressure requires work. You are working to get an intimate bond between two foreign products.
6. When one has completed the laminating process the next step is NOT to flood the veneer surface with finish or moisture of any kind. WOOD MOVES WHEN MOISTURE IS APPLIED. A barrier coat of sealer is recommended by a lot of the finishing manufacturers before your finish coats are applied. With the type of finishing you use make sure your first seal coat seals the wood fibers and does not flood the finish.

Good Veneering!

P.S. When veneer expands because of being flooded with finish, it sometimes takes about 3 to 5 months for the air-conditioner in a home to draw out the moisture. This is when the surface checks and blisters start showing up.

Locke Wilde, forum technical advisor



Buckling is caused by many things. To help eliminate it you can use a 2 part epoxy system like West System and vacuum bag it. It will take about 8 hours to cure. You can also use a polyurethane glue. It is a stand alone glue and you only need to apply it to one side and wipe the other side with a damp cloth before putting it together. You will also have to apply pressure to it to keep it in place until the glue cures. It can also be vacuum bagged.



Would you like to add information to this article?
Interested in writing or submitting an article?
Have a question about this article?


Have you reviewed the related Knowledge Base areas below?
  • KnowledgeBase: Adhesives, Gluing and Laminating: Glues and Bonding Agents

  • KnowledgeBase: Adhesives, Gluing and Laminating: Gluing and Clamping Equipment

  • KnowledgeBase: Veneer: Processing And Manufacturing

  • KnowledgeBase: Veneer: Techniques

  • KnowledgeBase: Woodworking Miscellaneous: Woodworking

  • KnowledgeBase: Knowledge Base




    Would you like to add information to this article? ... Click Here

    If you have a question regarding a Knowledge Base article, your best chance at uncovering an answer is to search the entire Knowledge Base for related articles or to post your question at the appropriate WOODWEB Forum. Before posting your message, be sure to
    review our Forum Guidelines.

    Questions entered in the Knowledge Base Article comment form will not generate responses! A list of WOODWEB Forums can be found at WOODWEB's Site Map.

    When you post your question at the Forum, be sure to include references to the Knowledge Base article that inspired your question. The more information you provide with your question, the better your chances are of receiving responses.

    Return to beginning of article.



    Refer a Friend || Read This Important Information || Site Map || Privacy Policy || Site User Agreement

    Letters, questions or comments? E-Mail us and let us know what you think. Be sure to review our Frequently Asked Questions page.

    Contact us to discuss advertising or to report problems with this site.

    To report a problem, send an e-mail to our Webmaster

    Copyright © 1996-2009 - WOODWEB ® Inc.
    All rights reserved. No part of this publication may be reproduced in any manner without permission of the Editor.
    Review WOODWEB's Copyright Policy.

    The editors, writers, and staff at WOODWEB try to promote safe practices. What is safe for one woodworker under certain conditions may not be safe for others in different circumstances. Readers should undertake the use of materials and methods discussed at WOODWEB after considerate evaluation, and at their own risk.

    WOODWEB, Inc.
    RR4 Box 265A
    Montrose, PA 18801

    Contact WOODWEB













  •   Home » Knowledge Base » Knowledge Base Article