Using glue instead of bondo to fill cracks for paint grade

2/18/15       
Mel Member

So you know how often a coat of primer can bring out a defect not quite that detectable by eye on naked wood?

Very time consuming correction for what it's worth if you ask me.

I was shown to sand down the product and shove bondo in there. A little problematic because bondo does not adhere to paint, and you can't quite sand paint out of a crack. so by the time you sand down the bondo I noticed that you often rip the bondo right out of the crack. I sometimes just skim it and sand smooth layer with 150 grit. But that still sometimes ends up with bondo being ripped out of the crack.

Now what if I used wood glue? Fill it, scrap off excess with putty knife then sand once dry. Nice viscous liquide that would fill the crack entirely just and stay there... And doesn;t require 3m mask to apply.

Any reason not to do this? I thought I;d ask first because I don't want to just try this thinking I'm oh so smart and end up getting returns down the line because I'm missing something.

2/18/15       #2: Using glue instead of bondo to fill ...
JM

just use wood filler, or what we use, DAP spackle.

No need for Bondo unless its a big chunk missing, in which you should have found this before you primed.

2/19/15       #3: Using glue instead of bondo to fill ...
Larry

The problem is adhesion. Inside of the crack it is almost impossible to get down to clean wood. Spackle will work if you can get paid quickly and don't want to do more work for them. Glue might work for a hair line crack but getting it deeply enough in to hold is difficult. Mask the area, put a bead of glue on the crack and use an air nozzle to gently force the glue into the crack. If the crack is a bit bigger follow with some sanding dust mixed with glue. There don't seem to be any perfect solutions other than ripping and re-gluing.

2/22/15       #4: Using glue instead of bondo to fill ...
Mel Member

Okay so I've since been going with the glue and pressing it down with a putty knife to ram it in there. Then I;ve been sanding before it's completely set to get a bit of sawdust in the mix as suggested. So far, so good. Faster then anything else I've tried so far, and it's been sticking. Feels like hackery, but working good!

On another note--I've been also using woodglue for mdf profiles. I was chatting up the painter who said she has a hard time painting the mdf end grain of profiles --eats an obscene amount of paint. So she suggested smearing it with glue and wiping off the access. Going good so far.

2/24/15       #5: Using glue instead of bondo to fill ...
Bruce H

I use super glue for this sort of repair. I'd spray some activate onto the surface and into the crack then apply glue and use a putty knife to force it into the crack. it sets up quick, a larger defect I use more super glue.

2/26/15       #6: Using glue instead of bondo to fill ...
Mel Member

Bruce, I tried this and man does it ever set fast. New rule of thumb for sure. Using masking tape as wood protector and spray adhesive and it sets in minutes. Brilliant.

2/27/15       #7: Using glue instead of bondo to fill ...
Jim Herron

Activator and super glue or autobody glazing.
Apply both sparingly as they both dry very quickly and are labor intensive to sand any excess flush.

3/8/15       #8: Using glue instead of bondo to fill ...
Adam

Muralo Pro Grade Spackle

This product is a gift from the wood finishing Gods. Every other spackle is inferior by a wide margin.

Muralo Pro Grade Spackle

3/8/15       #9: Using glue instead of bondo to fill ...
Adam

I have $60k kitchens that are 15 years old that I used Muralo spackle on. Many of those are waterborne. They are all still perfect. No cracking in beaded faceframes and shop made doors with applied miter moldings. This was all soft maple, birch ply, and a bit of mdf for door panels.

Like I said a true gift. We stopped using wood filler or bondo for anything less than a screw hole. Sand 150 grit, prime, spackle, sand 240, paint. No filling before the primer. The spackle blends perfectly into the prime coat. No need to reprime over the spackle.

3/8/15       #10: Using glue instead of bondo to fill ...
Adam

Mel,

Skip the glue on MDF. Try to use ultra refined MDF for a start it is less porous. Sand the end grain of the mdf with 240 grit. Brush BIN shellac or a catalyzed solvent primer on the end grain. Sand it with 320 grit. It will be as smooth as the face and no longer porous. We have done thousands of raised panels in mdf.

3/9/15       #11: Using glue instead of bondo to fill ...
Mel

Adam--no need to sand and reprime?? Wowsers. I like that. On it. Let you all know how it goes shortly.

3/9/15       #12: Using glue instead of bondo to fill ...
Adam

Mel,

I wrote a fair amount the other day.

Raised panels:
1. shape the profile
2. sand mdf end grain only 240 grit
3. spot prime end grain BIN or Clawlock
4. sand mdf end grain primer 320
5. spray the entire panel with primer.
6. sand the entire panel 240 grit
7. 1st topcoat, 320 grit, 2nd topcoat

Face frames:
1. use a decent amount of glue
2. sand the frames 150 grit
3. prime frames
4. fill all of the dark spots with Muralo Spackle
5. sand the primer and spackle 240 grit
6. 1st topcoat, 320 grit, 2nd topcoat

The old school way was to build your frames putty every defect you see(which is not many). Then prime it and then putty all of the spots you missed with a product inferior to spackle. Then you sand the putty off and generally have to reprime it.

Alot of wasted time. We've all heard of using sheetrock compound, bondo, and glue size. To solve the "mdf problem" the reality is all you need a fast drying sealer that hardens in the mdf end grain. Shellac and catalyzed primer fit that bill.

3/9/15       #13: Using glue instead of bondo to fill ...
Mel

Bah!! We are totally old school.

Told the painter today about your spackle. Her eyes got all wide and happy--she's got a can of it that she uses to fix mistakes when no one else is around. She's been telling people to use it for years. Set me off with the can and I'm widely impressed.

Will try the profile trick next time. Thanks for the very specific instructions, I love that.

The old school method is frustrating and time consuming. Happy to see other people nerd out on adhesives. Proper adhesives are most definitely your friend.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)