Compression bit yield on melamine

4/6/15       
Mike Hoffer  Member

Website: http://www.carolinaclosetsplus.com

We're using a vortex 3189xp 1/2" compression 2 flute bit and are only getting 15 sheet yield before getting chipping, etc.

I know the core has gotten crappier over the years but would love to hear if another brand bit would be better or maybe another melamine supplier. Currently we use funder commercial core

over the past 8 years, we've used lots of different brand bits. we used to get 50 plus sheets from roseburg but can't buy that anymore around here in NC.

any suggestions would be greatly appreciated. thanks.

4/7/15       #2: Compression bit yield on melamine ...
Larry

We've gotten very good yields from Onsurd Marathon bits. 3/8" 2 flute compression. 60 sheets of melamine+- mostly running Roucke brand. It has a better core than Roseburg.

4/7/15       #3: Compression bit yield on melamine ...
Mike Hoffer  Member

Website: http://www.carolinaclosetsplus.com

Larry, that's unreal yield. I wish we could get the same brand melamine you're using. We're testing to make sure our actual feed rates are what we have input into the machine. thanks for the info.

4/8/15       #4: Compression bit yield on melamine ...
Jason Scott

Have you checked to see if your tool gets hot or if your chips are warm right after cutting? It sounds like your chipload is off for some reason or other. Over the years I have also gotten batches of melamine with rocks in it that caused all kinds of problems with sawblades.

4/8/15       #5: Compression bit yield on melamine ...
Mike Hoffer  Member

Website: http://www.carolinaclosetsplus.com

Thanks Jason. yes, we've gotten some crappy melamine over the last year that had some trash in it. I think our speed/feed is correct. We're trying a different brand this week. We used to get 50 plus on a bit years ago.

4/8/15       #6: Compression bit yield on melamine ...
Mark

You are using a mortise compression for your thru cuts I see. This is not the end of the world, but if you have the flexibility I have found it much better to use a standard compression for thru cuts and the mortise compression only where it is needed. A lot better chip evacuation and less regrinding dust.
I think Jason and Larry are right, feeds and speeds may be off some.
Try 18000 rpm and 875 ipm for feed with these bits for melamine. It is a little faster feed than recommended, 720 ipm is more typical, but I still seem to get good cut quality. I get WAY more than 15 in both panolam and Tafisa, 60 to 80 densely packed sheets with an edge bander ready edge. What are you using for feed and speed now?

4/8/15       #7: Compression bit yield on melamine ...
Chuck Hicks Sponsor - Southeast Tool

Website: http://www.southeasttool.com

Board companies have figured out also that glue is cheaper than wood.

4/9/15       #8: Compression bit yield on melamine ...
Derrek

Call vortex direct and twlk to them. They have a new bit that we are using and are getting 50-80 sheets per bit and run at over 800 ipm. I have had off brand bits.that were.cheaper to buy but lasted only 10 sheets.
vortex gives you a break on purchase and sharpening if you send them 20 at a time. I buy 25 bits and send them 20 to sharpen At a time.

4/9/15       #9: Compression bit yield on melamine ...
Chris Boyer Member

Feed and speeds good suggestion - chip load and chip warmth good suggestion - invest in a infrared thermometer you can point at tool after it cuts , keep track of tool temperature. Another pointer often overlooked is weather the tool has been resharpened and by who. Most sharpening services would be lucky to have the technology needed to properly recondition today's complex tooling geometries. I always suggest to my customers that they send the tool back to the original manufacturer for sharpening.

4/10/15       #10: Compression bit yield on melamine ...
Mike Hoffer  Member

Website: http://www.carolinaclosetsplus.com

chris, what temp should the bit be if i get an infrared thermometer?

4/11/15       #11: Compression bit yield on melamine ...
Will Williamson  Member

Website: http://www.willmade.com

Touching with your hand means the tool is cool enough for you to touch it. Be careful you will burn your fingers. After that you will get the hang of it. When your fingers get close , you can feel the heat.
I've run vortex bits, till they did not even have an edge on them, but they were running cool and still doing the job, I guess they were just beating the wood off. not cutting at all.
I was cutting phenolic resin impregnated plywood 2 inches thick.Toughest stuff you will ever want to cut

4/15/15       #12: Compression bit yield on melamine ...
Phill

Mike,
You said you were trying a new brand of melamine. Good or bad result? If good, what brand? I've had our board rep and bit rep involved. Their suggestion to me was to go to a 3 flute 1/2" regular compression. I told them I was willing to try anything, so I have just started cutting with it. I'll let you know if I get a sustained better cut.

4/17/15       #13: Compression bit yield on melamine ...
Mike Hoffer

UPDATE:

Thanks a ton for everyone's input. I ended talking with Dan from Connecticut Tool who suggested an Onsrud bit - (#60-169MC, its a 2 flute bit with a 1 1/8" cut length and .562" upcut).

It's a standard compression, not mortise. After being educated from Mark on the post, we switched over. Results are amazing. We just got 53 sheets on the Onsrud bit. We're cutting white melamine 3/4".

We're also trying out a different brand white to see if that will help.

I haven't used the vortex version of the standard compression so it might work just as well. The real answer i think was going away from the mortise compression. I wish I would have posted this years ago. Thanks to this forum, I'll save $$$$$ with the correct bit :).

Connecticut Saw & Tool
140 Avon Street
Stratford CT 06615
(800) 404-1220
(203) 378-7346 (fax)
www.ctsaw.com

4/22/15       #14: Compression bit yield on melamine ...
R4G3X Member

Congratulations on the upgrade to a standard compression, guaranteed you will see much better performance from it. From what I've seen most people get about 60 sheets so its average with these bits in laminate particle board. In the beginning, examining the tool every 10-15 sheets will tell you a lot about how well your machine has been tuned.

I haven't tried the Onstrud marathon bits yet but heard they people are getting 100+ sheets.

You also need to look at the size of parts you are cutting, as that will affect the number of sheets per bit. Larger parts (closets) will yield much sheets per bit more verses smaller parts. You really shouldn't see any chipping, even at 100+ sheets I have never seen any chipping on either side of the material ever, even with a dull bit. My guys change the bits when feel they are dull and need sharpening (you can hear it).

Here are some suggestions to get even better tool life from your new bits.

Run an air hose (better yet 2) and point them at the end of the bit and turn them on while it is cutting (if you havent already done this and if you have the compressors). You should see a huge difference by doing this.

Keeping the bit (like with a resin cleaner) clean, and it only takes a few minutes. Resin on the tool creates excess friction and heat that will quickly reduce the tool life.

Lastly but most importabtly be careful with the feeds, speeds and chiploads given to you by the tool manufactures, these serve as a STARTING point only. Every machine is different and needs to be tuned accordingly, this alone can extend the life of the tool beyond most people will tell you is impossible. I think its Onstrud that has a very good guide for starting out and learning to adjust these. It's a very good read, maybe give to your operator/programmer, but again it's just a start.

Hope this helps, best of luck in the future.

Michael

4/24/15       #15: Compression bit yield on melamine ...
Rob Long

We use an Onsrud 3/8" compression with the marathon coating. We cut a lot of laminated panels as well as melamine. I can get 65-70 mixed sheets melamine and pre-laid sheets per bit. Im cutting out of 5x8 and use a duramine product.

5/2/15       #16: Compression bit yield on melamine ...
Larry

Use MDF melamine.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Onsrud Cutter Vortex Tool Company T-Tool USA Limtech Industries, Inc.