Rub Throughs

3/26/18       
John Bishop  Member

Website: selectwoodworking.net

It seems like no matter how careful I am I will still break through the first sealer coat and kiss the stain or dye coat.

I am a sander that’s for sure. Have allways believed the first and second coats being flat and clean are critical to the success of the project.

Especially on tops we sand the first coat very aggressively to get it flat and no matter how careful allways seem to break through in a few spots. I am wanting to try to spray my first coat than not touch it at all between coats. Let it dry than second coat in hopes of getting enough build to avoid my breaking through. Has anyone tried this or do you have any other suggestions on this??

Sealer for tops is ML level sealer. It goes on heavy and wet. My first sand is with mirca gold #400 grit. If it’s a top I use a DA with a 3M soft interface pad. Being very careful at edges. I get the same break through when hand sanding that first sealer coat by hand because I want it perfectly flat. I think it’s a curse.

Since I sand so much I put on 3-4 coats of level sealer to get a nice filled look always mindful of maximum total finish thickness of compleated system to avoid an excessive film build and a failure.

Top coat with CV. Allow try and buff. Do you level sealer folks thin that product ML says not too and we do not but when it’s chilly in here the results are frisky since the level sealer is so heavy. I understand it’s made to be sprayed like that and it will not shear and atomized properly if thinned. I’m just curious if anyone has tried.

Thanks for help

DJB

3/26/18       #2: Rub Throughs ...
Mastercabman

How about sanding not so aggressively?

3/26/18       #3: Rub Throughs ...
rich c.

I'd suggest you play with thinner and nozzle size so you don't have to sand so aggressively. I get real gentle near the edge on the first sanding. Maybe even leave it a little short of perfect to prevent the burn through.

3/27/18       #4: Rub Throughs ...
JeffD

I suggest not "sanding" between coats as just thinking that your sanding has you in the wrong place. What you want to do is "scuff" between coats. Just applying an even scratch pattern to the full surface and removing any little nibs. Your not, (or shouldn't be), trying to flatten the surface between coats, it's already as flat as its going to be at that point, your just removing any defects and giving the second coat something to "bite" into. If you approach it like that you'll have few if any burn throughs.
Trying to flatten each successive coat is not only a waste of time and material, it's also reducing your overall build thickness. I learned this years ago the hard way sanding polyester finish on boat parts. It did not go over well when I had to go to the boss with parts that I had rubbed through the finish!

Only once you have all the coats on do you want to sand the surface thoroughly if your going for that rubbed out finish.

good luck,
JeffD

3/30/18       #5: Rub Throughs ...
DanShaf Member

Sand with 320 grit, random orbital sander. Don't use the soft interface pad for sanding. You need a stiff backing pad.

There are two reasons to sand between coats, each of them different. You sand because you (1) as a corrective measure, to subtract from what you've sprayed, or (2) you only need to create a tooth for purposes of intercoat adhesion.

To use a soft interface interface pad for corrective sanding is like shoveling wet sand at the tidewater mark on the beach. Using a grit that is finer than 320 for corrective sanding only burnishes your finish, it doesn't have enough grit to be subtractive enough, (the corollary is that 220 or 240 is way too course and it will etch in too deep of a scratch pattern). Go with 320 for corrective sealer/primer sanding.

We also scuff to a smooth surface when sanding between coats. Start smooth to have your best shot at staying smooth.

The soft or mefium interface pads are great for Abralon and for scuff sanding but not for level/corrective sanding.

4/2/18       #6: Rub Throughs ...
Bill  Member

Website: canadianacabinets.com

Are you putting a good break on your edges
before finishing? Also the sandthrough to the base is what would be there if it had worn naturaly. Maybe trying too hard as sandthrough is an attempt at replicate natural where.


View higher quality, full size image (4300 X 3088)

4/3/18       #7: Rub Throughs ...
John Bishop  Member

Website: selectwoodworking.net

Thank u much to all. I am a recovering sand aholic 😁. The first step is admitting u have a problem. I believe I sand too much between as many mentioned. Going to try scuffing more between to maintain film build. Then I can get it on after a good film build and level that. Much happiness getting to sand flat.

Plan on trying abralon also. In past had problems sometimes when rubbing to a dull sheen it will burnish a bit from hard objects. Cuff buttons, finger nails and such. I have never succeed in finding a work around for this. Has anyone had luck in this area? In my part of country Ohio we don’t seem to do much shinny work.

4/5/18       #9: Rub Throughs ...
jay

a lot of it is how you hold the sandpaper. also try using the square sanding sponges. (the thin ones not the big thick ones) and just kind of wrap it around your hand so that as you sand the edge isnt dragging on the corners


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)