Subject: Re: checks in maple paper backed veneer doors

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

checks in maple paper backed veneer doors

12/31/14       
Earl Member

I have some small checks showing up(along grain and slightly raised) on maple paper back veneer doors 3 months after finishing doors.
Door mfg specs are as follows:
core 3/4" mdf edged with 3mm solid maple, glue hand rolled helmetin 416 PVA, 10mil paper back maple veneer used front and back of doors (total thickness 28mil paper and maple)

Procedure:mdf is edgebanded then glue is hand rolled on to mdf and the veneer and is immediately pressed in vacuum press at 18hg and heated to 80C for 2.5 minutes. The RH at press time was 45 to 50% and is now 30 to 35%. doors sat in shop for about 1 week before being finished with spay stain and converted varnish.
Veneer is tight to core and when veneer is ripped off core paper remains stuck to core and veneer (paper separates).

I am looking for input as to what is causing the checking. Is paper back veneer a good choice or is fleece or raw veneer a better choice??? Want to used veneer type with least chance of problems.

ps I also made some sample doors at the same time as checked doors and are still unfinished with no signs of checking.


View higher quality, full size image (3264 X 2448)

1/2/15       #2: checks in maple paper backed veneer ...
Charles Wright  Member

Website: http://www.northcreekwoodworks.com

Hey:

Guess #1- Poor bond between paper & veneer. If you have a vac press why not use unbacked veneer? Rolling glue is OK but make sure you use the min amount, Check with a wet mil gauge (get one from your glue supplier).

Guess #2- Too much finish. Measure dry mil thickness and check with your finish maker.

1/2/15       #3: checks in maple paper backed veneer ...
Earl Member

I am new to the whole veneering world but not to wood working. Press has been used for thermal wrap up til now. In our testing we used raw and paperback , the raw tested was deeply pocked similar to birds eye chipped on a planer and took for ever to palm sand out .( is this the norm for maple veneer or any type of veneer??)
Paper backed was recommended to us as a better product less issues and was so easy to work with sanded already etc. As i research more it appears there is more long term problems with paper back????( looking for feed back on long term issues paper back vs raw as in my process ).

Is there any good literature or links on veneering using heated vac press pva glue humidity??

1/2/15       #4: checks in maple paper backed veneer ...
Charles Wright  Member

Website: http://www.northcreekwoodworks.com

Sounds like you got a bad batch of raw veneer for your testing.

1/2/15       #5: checks in maple paper backed veneer ...
Dave L

Raw veneer has what I call plus and minus grain. The tight/good side has some high grain and the back side has some low grain. With good quality veneer, the sides are really hard to tell apart. Worst case is lots of high grain on the front and "deeply pocked" grain on the back. The only maple I've gotten that had significant +/- grain was some highly figured western.

What was the moisture content of the veneer and substrate before you started, had they both had time to acclimate to the 45 to 50% environment? Since the RH went down and you have puckering, instead of splitting, the core had to have shrunk more than the veneer. Either the core had a higher moisture content before pressing, or it expanded more/absorbed more moisure during pressing.

I have no idea how heat affects the process. Is a heated platten in direct contact w/ the veneer, could it drive moisture out of the veneer and into the substrate?... Is the temperature enough to affect the bond between paper and veneer?

In my experience with PVA cold pressing at >= 20hg for 1/2hr with 1/4" MDF cover sheets, splitting would be more likely. My single side layups always dry flat or cupped on the veneer side, i.e. the glue/veneer contracts more than the substrate.

I wouldn't think a 15% change in RH would be enough to cause that puckering unless there was, at some point, a significant difference in moisture content between the materials and/or there was a pretty weak/non existant bond between two of the materials.

1/2/15       #6: checks in maple paper backed veneer ...
Earl Member

The core and veneer would have been in the shop for about a week before processing and week to process .

I do not have a moisture reading for veneer or the core.

The rep from the mill that layed up the veneers and applied the paper told me the temp that i am using would not affect the paper bond. The only way i tested the bond was to rip the veneer off with a pair of pliers and in that test the paper separated leaving paper bonded to veneer as well as the core. The veneer came of in small pieces .

The press heats the silicone membrane that i place a piece of 70lb craft paper between veneer and membrane.

PICTURE BELOW :
I took a piece of 1/4" mdf maple front and back (factory ) and glued a scrap piece of paper back maple veneer to it at 90 degree to grain on the 1/4". Use same glue and heated vac as posted before, 1/4"and veneer applied were in shop envirment for months. Then i had it stained and finished with converted varnish ( same as doors). This picture show what happened to it in about 6 weeks (RH same as posted before) by the way the 1/4" is not cupped. This was done to test glue finger print to see if we sanded printed away.

I included this picture thinking it may tell you experts something more about the checking as it is on a different core that had been aclimatized for several months.


View higher quality, full size image (3264 X 2448)

1/3/15       #7: checks in maple paper backed veneer ...
Robert Member

What was the finishing schedule.

1/3/15       #8: checks in maple paper backed veneer ...
Earl Member

Re finishing schedule : our shop did not finish the doors or the 1/4" sample above but i will tell what i know about it. Doors were finished about a week or so mfg. they were spray stained with solvent base stain (no wipe) chem craft hawaiian tan. Then strayed with conversion varnish (chem life 24) dont know how many wet coats (i think he said 2 but not sure) or time between coats.

I took a sharp knife and cut some veneer and varnish off at a sharp angle then measured the cut piece with digital caliper at the point where stain and conversion varnish met it measured 4.5 mil . Did this 3 times and got same results each time.Not sure this is the right way to measure dry finish thickness but makes sense to me it would be accurate .

1/3/15       #9: checks in maple paper backed veneer ...
Dave L

I'd do two samples, one with a waterbased finish and one with paperbacked from a local box store, i.e. change one potential culprit for each sample.

The only time I've had veneer pucker like that was when I glued paperbacked with contact cement. It was my first veneer job and I haven't used either since.

1/3/15       #10: checks in maple paper backed veneer ...
Charles

1- Ask the finish supplier what they think, now that you know the dry mil thickness. No one here can answer unless they know the actual composition of the finish

2-Cross cut a sample 90 degrees to the checking and use a strong magnifying glass to inspect. You should be able to see what in fact is checking or loose.

1/3/15       #11: checks in maple paper backed veneer ...
Brian T

I have had the same issue but the checking shows within 24 hrs of the finish drying. It's not normal checking it's the reaction between the finish and the glue under the paper and veneer. The only sure resolution I have found is to use to wood backer.

As the finish dries it creates tension or pullback which lifts the veneer away from the paper. The paper is thin and the finish was able dissolve the bond between that and the veneer which weekend the bond enough allowing this to happen.

I have had seen this happen with water and solvent based products but always with a paper backed veneer.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)