I have been having issues when gluing up radius jambs. They seem to cup on me. I am not talking about springing, cupping.
I make a form then lay up 1/8" to 1/4" skins and clamp them to the form. After the glue dries and I remove them from the form they have a cup to them. Can anyone give me some insight on this.
Thanks

10/23/18       #2: Gluing up radius jambs ...
David R Sochar

Width of jamb? Glue type? How many laminations? Radius?

10/23/18       #3: Gluing up radius jambs ...
Peter Smith Member

David, Jamb width varies, but most are around 6 to 9" wide. Glue is loctite UR 5153 Polyurethane. The lay up was (2) 1/4" (1) 3/8" wiggle and (2) 1/8" in that order with the 1/4" oieces being the inside face of the jambs. Radius on the last piece was 240"

10/23/18       #4: Gluing up radius jambs ...
DOM

Are you using male AND female forms?

10/23/18       #5: Gluing up radius jambs ...
Peter Smith Member

DOM,

We only use the male form and wrap the skins around it and clamp them with a non glued skin and blocks over that.

10/23/18       #6: Gluing up radius jambs ...
DOM

Im not a fan of that Peter. I always make both. If you dont have a CNC machine i know its alot more work but so is remaking the jambs. I used to use truck straps before i hit myself in the head enough times.

10/23/18       #7: Gluing up radius jambs ...
Peter Smith Member

DOM,
Some of these jamb units are 8-10' long so making a male and female form gets crazy. I do have a cnc machine. If using both eleminates the cupping I will do that. Thanks for the input.

10/23/18       #8: Gluing up radius jambs ...
Fred

Website: http://www.rivercity.ca

Hi Peter,

Do you apply glue to both surfaces on each joint or only one side? If you only apply to one side perhaps those sides in each layer get a chance to take on more moister prior to clamping. As a result each layer dries more on one side and the whole jamb cubs?

10/23/18       #9: Gluing up radius jambs ...
Peter Smith Member

Fred,
Both sides are glued evenly. We roll the glue on oneside lay it on the form, then roll the glue on the face side. When placing the next skin on we roll glue that as well and lay it on the glued face side of previous skin.

10/23/18       #10: Gluing up radius jambs ...
David R Sochar  Member

More Info Request: How much cup? 1/16" or 1/2" Across the entire width and length, or just in spots? Is Loctite a solvent based glue - no water?

10/24/18       #11: Gluing up radius jambs ...
Tom Gardiner

The glue is not the likely source of moisture as it is PU. I would use a moisture meter on the skin stock. If you are resawing for the skins then it is likely that the core of the stock is wetter and is cupping when exposed to the atmosphere. The cure, check the moisture of the stock. Resaw and let skins acclimate before use.

10/24/18       #12: Gluing up radius jambs ...
Peter Smith Member

Tom,

Thanks, I will try that as we do resaw then sand them and lay them up. I will let them sit for a day or so and then glue up.

10/24/18       #13: Gluing up radius jambs ...
Fred

Hi Peter,
I may have misunderstood your layout of the lamination layers.
You have 2 @ 1/4" on the inside of the Jamb
Then @ layer of 3/8 bendable ply and 2 @ 1/8 on outside of jamb?
If this was the sequence the different layers inside versus outside potentially create the cop?

10/24/18       #14: Gluing up radius jambs ...
Peter Smith Member

Fred,

We thought that as well. We will not be doing that in the future. Thanks for all your input. We will be taking all the information we have from here and putting it to use.

10/24/18       #15: Gluing up radius jambs ...
John Member

I think your unbalanced construction might be the source of the problem. Separately, I put curved jamb laminations in a narrow vacuum bag I made and clamp it into a female mold.

John

10/24/18       #16: Gluing up radius jambs ...
Gary

I put a 1/16" flat steel band ( same width as jamb) over the male mould first. Then all the laminations followed by 1/16" steel band last. I would get rid of the wiggle wood and stick to solid wood laminations. I also would use Resorcinol or Plastic Resin Glue as it cures COMPLETELY RIGID. Male and female moulds are the only way to go. EASY to clamp as well.

10/25/18       #17: Gluing up radius jambs ...
Adam

My first guess would be uneven clamping pressure. I suspect you are bending your cauls. You get more clamping pressure on the edges of the laminate.

I did many many curved/radius jambs for my first boss. We always seem to get all of the radius topped doors and windows.

Our method was farm tech. 3/4" plywood sides in the shape of the inner curve. poplar sticks screwed from one side to the other. first layer was something flexi & smooth like masonite. Then poly sheeting. Throw the layers on glueing them with epoxy. Stiff poplar cauls on top of the laminate. Nothing to smooth out the clamping force. We had 5/16" carriage bolts as clamps in each caul.

Other than caul marks on the outer veneer these jamb sets were perfect. What are your cauls and clamping force?

I've never seen a laminated jamb cup. Excessive spring back and delamination are common.

10/25/18       #18: Gluing up radius jambs ...
Peter Smith Member

Adam
Cauls are either sapele or poplar. We use I-beam clamps. The form templates are made on the CNC with offset openings for the clamps to fit in. These jambs are for garage door openings, so they are typically large in length. (When we door man door jambs we haven't had any issues.) We have had success and we have had cupping. Usually the cupping is about 1/8 to 3/16". I am just trying to figure out the best method so we can be consistent. The feedback we are getting here is great and I hope to put it all together to come up with a successful plan of action. Thank you for your input.

10/27/18       #19: Gluing up radius jambs ...
BH Davis  Member

Perhaps I missed it but you don't seem to have specified which way these are cupping. Are the edge curling up towards the face of the jambs or rearward towards the back of the jamb.

I.e. is the face of the jamb concave or convex across the width.

BH Davis

10/27/18       #20: Gluing up radius jambs ...
John Member

The most uniform pressure possible is with a vacuum bag, and you only need one form. You don't even need a complete form, just enough points along your arch to define the shape. See attached photos.

John


View higher quality, full size image (3648 X 2736)


View higher quality, full size image (3648 X 2736)

10/27/18       #21: Gluing up radius jambs ...
Adam

Peter,

Your fabrication methods are excellent.

Glue really has little impact. We use epoxy 95% of the time, because of the working time, we have buckets of it, and it’s waterproof. Titebond1 works fine if you are fast. Needs two guys.

The problem is your laminate schedule. It should be balanced. We use 1/4” veneers of the same wood sanded to 80grit on the thickness sander.

I’d guess the bending ply is 100% of the problem. 1/2” wood, 3/8 bending ply, 1/4” wood is as unbalanced as a laminate can get. You are also wasting time & material for zero gain.

We’ve done 2 car garage doors 12” wide layups with zero cupping. That was with the farm tech method. We have used a similar method as yours for the last 15 years.

BH Davis specialises in curved/radius work. I would take his opinion over anyone else’s including mine.

10/27/18       #22: Gluing up radius jambs ...
david zaret Member

john, can you talk a little about that bag setup - is that a disposable, one-time use bag, or one you use repeatedly? can you point me to the material/vendor (assuming it's a one-time use)?

thanks.

10/28/18       #23: Gluing up radius jambs ...
John Member

Dave, I made the bag from 30 mil vinyl that I bought at a local shop that makes custom boat windows, covers, etc. McMaster Carr sells it, too. Vinyl is PVC and can be glued with regular PVC pipe cement, or a special PVC glue you can buy from Joe Woodworker. You also can buy bag penetrations from him, as well as seamless vinyl and polyurethane bag material.

You don't need any special closure system although you can buy them. I just roll the open end of the bag around a piece of wood and clamp another over the top. The vinyl sticks to itself well enough that it forms a very good seal.

Polyurethane is more pliable than vinyl and more durable, but I'm cheap and a low volume guy so I use vinyl. I'm still using the first bag I made over 20 years ago and it has been used probably 100 times, with just a couple of leaks that were easily patched.

No matter how you go about it, a vacuum bag is the easiest and best way to get uniform pressure on anything curved, or flat for that matter. I've done a lot of curved work, including some pretty large panels, and only having to build one mold greatly simplifies the process. With curved head jambs you put the laminations in the bag, pull a slight vacuum, then clamp it against the mold with cauls on the non-mold side, then pull the final vacuum. I use thin plies, rarely more than 3/16", or bending plywood sometimes, and plastic resin glue or epoxy to eliminate spring back.

John

joewoodworker.com

11/1/18       #24: Gluing up radius jambs ...
AM

Liking our curve-o-matic. Been doing this a long long time and have tried every method mentioned here. Vacuum bag for us is to cumbersome and not accurate enough for door work especially large full round. Male female is ok but the stars have to align perfectly to get even clamping pressure. Prior to the curve-o-matic a male with thin layers of solid wood and multiple caul layers, strap clamps, was the best. Our rule of thumb is if it doesn't lay over the form easily the lams are too thick!


View higher quality, full size image (640 X 480)


View higher quality, full size image (640 X 480)

11/2/18       #25: Gluing up radius jambs ...
Pat Gilbert

http://www.curvomatic.com/

http://www.curvomatic.com/


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Doucet Machinery ExFactory