Wilsonart 1731 adhesive delamination problems

10/8/15       
Richard Member

About a year and a half ago we switched to Wilsonart 1731 spray adhesive. Now we are having calls for counter tops and cabinet doors where the laminate is just falling off. We have been in business for 25 years and never seen anything like this. Was wondering if anyone else was having this problem?

10/8/15       #2: Wilsonart 1731 adhesive delaminatio ...
Jeff Pitcher

Richard,
While I can't speak directly to the Wilsonart product, I did notice that this is their VOC compliant product based on methyl acetate. My experience with similar products has been problematic at best. It's not that there is a problem with the adhesive but it works differently than traditional contact cements. If the operators are unaware of this you can see considerable de-lam. The products I've seen issues with have a very short open time because of the "compliant" solvent. Operators are used to having 1/2 hour or more to put the pieces together. I've seen methyl acetate based products exceed their open time after 5 minutes. Unfortunately, it appears that everything is bonded okay but it's really a very cursory bond. This may or may not be the case with the Wilsonart product but it is definitely where I would start.

10/8/15       #3: Wilsonart 1731 adhesive delaminatio ...
Richard Member

Yeah we have had a glue rep in here and they said it was our spray pattern. If the glue is that temperamental then they should properly show how it needs to be applied. Does anyone know where the Wilsonart 1731 is manufactured?

10/8/15       #4: Wilsonart 1731 adhesive delaminatio ...
Robert Member

Wilsonart adhesives plant is in Temple TX next to the laminate plant.

10/8/15       #5: Wilsonart 1731 adhesive delaminatio ...
Robert Member

LOW VOC Methyl Acetate Glues are very different from traditional contact cements. The air pressure and fluid pressure has to be less. ( it should be on the tech data sheet) They atomizes very well. This helps with any telegraphing that may be caused by the "FAT" pebble pattern of traditional contact or the "WEB" pattern made by canisters. BUT, if the air pressure is too high then the glue can dry before it is even touches the laminate or board. This also makes for a pebble pattern that is very small. So, to make "CONTACT" proper pressure is a must. No longer can you get away with blocks of wood, hammer and block, flooring rollers, or your bare hand. 3" J rollers or pinch rollers should be used to get the "PIN POINT PEBBLES" to touch each other and make good contact. Once the glue contacts more individual places the bond is incredible. I would put it up against any traditional contact cement.

10/8/15       #6: Wilsonart 1731 adhesive delaminatio ...
Jeff Pitcher

Great information Robert! I would definitely agree that there is no inherent problem with the glue. It's really more a matter of proper training and a full understanding of how it's different than the traditional stuff.

By the way, would you suggest using it for veneering? :-)

10/9/15       #7: Wilsonart 1731 adhesive delaminatio ...
Larry

A better solution is water based contact. Not temperamental about short open times. It just needs to flash off long enough to not leave water behind. That is longer than traditional solvent based. That isn't a problem. You just work on a few more parts at a time with not labor cost increase. We've been using the Henkel product for many years. Greatly reduced health risks! It is different to use. So learn how first.

10/9/15       #8: Wilsonart 1731 adhesive delaminatio ...
Robert Member

Larry,

Henkel makes a Water based contact cement? What is the name and number on it. thanks

12/7/15       #9: Wilsonart 1731 adhesive delaminatio ...
JIM

We also have been in business for 28 years, switched to the low VOC glue and two tears later the laminate is falling off and curling up. We laminated both sides of our doors with the glue and only the exterior of the doors are falling off. Explain that?

12/9/15       #10: Wilsonart 1731 adhesive delaminatio ...
Robert Member

JIM,
I have seen that with LOW VOC glues coverage and pressure are key in the bonding ability of the glue. If you have the laminated panel in a place were the laminate is going to grow and shrink quite often, then 100% coverage and 30psi is required. A pinch roller or a three inch "J" roller is recommended. No longer are blocks of wood or flooring rollers acceptable. Perhaps the exterior side had more fluctuations with moisture causing the laminate and substrate to move. This caused the glue to sheer and break.

I am only guessing here. But, you asked for an explanation. I could never know what happened in your case after reading one paragraph. I hope this helps.

12/10/15       #11: Wilsonart 1731 adhesive delaminatio ...
Gene Wengert-WoodDoc

An inspection by a qualified person will likely give us the reason for delamination. However, we know, and stated clearly in the above postings, that these low VOC and non-F (or minimal about of "F") adhesives require different procedures for application, different MCs, different pressures and so on. In fact, I provided that info to the EPA regarding the potential to switch from the "F" adhesives. I agree with Jeff, that the newer adhesives are indeed excellent; it is the application techniques where we have issues at times.

Regarding doors, we do know that the exterior side of a door has larger moisture content changes than the interior. This means that a glue joint on the exterior side will have to be stronger than the interior side to prevent delamination. So, if we are making a reasonable joint, but it is not as strong as needed, the exterior side will fail first.

1/19/17       #14: Wilsonart 1731 adhesive delaminatio ...
Naomi

We are having the same problem with delaminating. When we were thinking of switching to the product we were told specifically by our supplier that the process we used to apply the adhesive was sufficient for the glue. The specifications say to apply with 40-50 psi, which we are definitely doing. Now, two years later they are blaming our process for the delaminating, just as it sounds like the rest of you are experiencing. We have older projects (8 years old) where the same product is not delaminating, but the new projects where we had a different lot of the glue (2-3 years old) are delaminating. It seems that when the weather turns and gets drier we get notification from our clients. We also went to one client last year to test their laminates and found them securely attached without issues, and then just a few months ago the product is now delaminating. This is costing our company significantly as we are repairing these laminates under our warranty. We believe there was a bad lot of adhesive. We have documented all of this, and plan to file a consumer protection complaint. If anyone is interested in also filing a complaint, feel free to contact me for more info.

1/20/17       #16: Wilsonart 1731 adhesive delaminatio ...
Dave

Can anyone say "Class Action Suite", and would you be willing to join? There is a law firm in Virginia representing a cabinet shop having huge exposure from using this adhesive over the past couple of years. I have his name and number if anyone is interested. We used this product for a little over 2 years and started receiving delamination phone calls at about the 1 year anniversary, or when the building cycled into the heating season. To date, we have had over $50,000.00 in out-of-pocket labor costs because many of these repairs need to be done during off hours and we have had to purchase several thousand dollars of replacement laminate and a glue solution to fix this issue for our customers.
Wilsonart is playing the "it's your fault" card with us and 2 other larger shops in our area, like we all forgot how to spray contact cement one day. Our local glue supplier has gone silent and rarely visits our offices anymore. Maybe a law suite will get their attention.

1/23/17       #17: Wilsonart 1731 adhesive delaminatio ...
Unstuck Member

I really want to learn the names of other shops with 1730/1731 issues. We have almost $3 million in work out there that's being held together, or not, by 1730. In the past 2 weeks nearly $150k of work has been reported as delaminating.

1/27/17       #18: Wilsonart 1731 adhesive delaminatio ...
Rob

Just like everyone else, we're going through the same thing. Seems like every week, I get a call about another project. My rep (Wurth Wood Group) has brought the WilsonArt glue specialist by and he said without sending a sample for testing, they can't tell. Some of the pieces are clearly application errors, but when there is 90% coverage, with no shiny areas, and some substrate actually coming off with the laminate, then that's not an application error. We've switched to StaPut SP80 canister to eliminate any human error, but we have 2+years of projects out there with the 1730. Prior to that we used the DAP low VOC and never had any problems. Wurth told us their glue was better, cheaper and would use the exact same pogo pump setup. Nothing needed to change. That definitely hasn't been the case. We would love to get information on any class action lawsuit, since we're not getting any help from our rep.

4/11/17       #21: Wilsonart 1731 adhesive delaminatio ...
Angela

Website: http://cherryworksltd.com

We have also recently had problems. Every other day I am getting calls that things are delaminating from 2 1/2 years ago. We started using the glue about 4 years ago and had no problems with those jobs. I have almost $10,000 in labor repair costs at this point. We have been in business for over 40 years. Never had a problem like this. Same story as everyone else. We all may have to get together on this. I don't know how many other projects are going to come up.

2/9/18       #31: Wilsonart 1731 adhesive delaminatio ...
Jeff

We are a small fabricator in PA and in the last 2 months have had to fix six jobs that were fabricated in 2014 using 1730 wilsonart glue. We have been in business since 1974 and the only time we have had delamination problems was with wilsonart blue glue. We all know that product resulted in a nation wide law suit.

2/9/18       #32: Wilsonart 1731 adhesive delaminatio ...
Andy

This is a wilsonart problem. Talk to your wilsonart rep. We have projects with both 1730/1731 d-laminating. All 2 to 3 years old.
I believe wilsonart had a hard time trying to reformulate their adhesive to meet CA new VOC regs. I just love the government. Anyways, we have been getting payment from wilsonart for fixing these issues. It is a pain in the ass as we keep going back to the same jobs as new d-lam occurs. We invoice wilsonart each time.

2/15/18       #33: Wilsonart 1731 adhesive delaminatio ...
Naomi Kroth

Seems that the Wilsonart payouts are pretty selective and a paperwork-heavy process, but for those really taking big hits to repair all the d-lam such that their company is in jeopardy its worth the time. But you have to make a lot of noise to get tapped into the payment process. FYI I also know there are a couple law firms looking at this issue. They've been made aware of this thread and I think would contact everyone here if they plan to pursue something, but at the moment nothing is being promised litigation-wise.

7/17/26       #36: Wilsonart 1731 adhesive delaminatio ...
Andy Clifford

I have been installing laminate countertops for 26 years. I started using W/A 741 spray adhesive spring of 2023. Started getting calls of delaminating spring of 2025. I now have 14 jobs delaminating. Almost all from 2023 and now a couple from 2024. W/A rep is giving me the same bs. Seems like they still haven’t fixed the problem. Anyone else still dealing with this? Did any lawsuit happen with the 1731?

7/17/26       #37: Wilsonart 1731 adhesive delaminatio ...
Robert Boutin

1. 740 is a totally different adhesive than 1730
2. 1730 was never found to be faulty.
3. Have you contacted your Wilsonart adhesive rep?
4. Has your Wilsonart rep sent any samples to their lab for testing?

7/17/26       #38: Wilsonart 1731 adhesive delaminatio ...
Robert Boutin Member

Sorry,
I just read where you said the WA REP gave you the same BS.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • Vacuum Pressing Systems, Inc.
      Vacuum Pressing Equipment - Including Bag and Frame Systems
    • ULTI-BOARD
      The Ultimate Spoilboard - ULTI-BOARD - Specifically Engineered and Formulated for the Ultimate in Spoilboard Performance - Not Your Ordinary Sheet of MDF.
    • Excel Dowel and Wood Products Inc.
      Plain and Pre-glued Dowel Pins, and Wood Parts - Servicing Small Hobby Shops to Large OEM's
    • Rangate
      Woodworking Machinery, Supplies and Knowledge

    Become a Sponsor today!