2/11/17       
Larry

Just had a small (3/8 x 7 x 7") clear acrylic panel returned to us. It was part of a decorative front on a teller line. It had severe internal cracking radiating from each standoff hole. The teller line had been in use for 2 months. Customer said all five were fine when they left but next morning the panels were all cracked except for the 6th one that was mounted high on a wall decoration. They were unhappy and accusing.
I'd never seen this before. Time for research via Google. Alcohol was highly suspect. We did a test on the one hole that was unaffected on the returned panel. We had put washers and bolt/nut in the hole to duplicate the attachment. Apply liberal amount of alcohol, it took less than a minute to start showing cracks and in five minutes they had spread 2".
The savings and loan company had probably changed cleaning contractors and they likely used a cleaning product with an alcohol base.
There are acrylic faced panels being used for door and drawer fronts. If you use any, warn your customers about this. I didn't know about it. Did you?
PS the face of the panel was unaffected other than the cracks.

2/12/17       #2: working with acrylic ...
MarkB Member

If you google acrylic cracking alchohol you'll find endless info. We do a bit of acrylic sign work and have read about it extensivvely over the years. Windex or most general window cleaners are a death sentence. I think there is even a video around showing the cracking in real time after flame polishing an edge.

Hard part I could imagine in a commercial application would be once you let the customer know how dangerous the problem is they may avoid the material. I'm not sure if with drilled holes you could've gasketed the cleaner away from the raw drilled edge with a rubber washer on both sides.

2/13/17       #3: working with acrylic ...
Alan F.

Do you provide a use and care manual at the end of each job? Lumicor in my sample is an acrylic.

A-

Click the link below to download the file included with this post.

Sample_Care_and_Maintenance.pdf

2/13/17       #4: working with acrylic ...
Larry

Many commercial sites use cleaning services with multiple crews. It would take a very dedicated store or office manager to make sure everyone of the crews understood enough English to understand the problem.
Alan, nice for the items generally used. Do you send it with the shipment or mail directly to the store c/o the manager?

2/13/17       #5: working with acrylic ...
Alan F.

Larry, we have a library of about 50 items, we built the instruction based on what materials are in the job. We submit it with the warranty. If it a real heads up material we put a label in the cabinet or on the product.

For our work which is commercial the GC turns over the manuals to the owners who give them to cleaning companies and staff.

We will also put "LOOK" on the shop drawings to anything with special care.

Generally our assistant puts the use and care together from the shop drawing spec page and inserts the items used from the library. If there is a new item she gets the use and care from the manufacturer and adjusts the instructions if need be for me to review.



Click the link below to download the file included with this post.

Document1.pdf

2/13/17       #6: working with acrylic ...
Larry

Thanks Alan.

2/15/17       #7: working with acrylic ...
Larry

Follow up information. Extruded acrylic does the craze thing, cast does not. Also the edges have to be heat polished for it to happen. We did a test run and found it to be true.
Used to be cast was a lot more expensive, not true now. It is more variable in thickness but for what we use it for, doesn't matter. Only cast from now on. We also use a lot of PETG for grocery store work. much better durability than acrylic. Heat forms nicely.

2/16/17       #8: working with acrylic ...
Pat Gilbert

Larry

Just out of curiosity how are you heat forming this material?

2/16/17       #9: working with acrylic ...
Larry

For PETG we have the typical strip heater to do angle bends and also have an oven for larger parts up to 3 x 8'. Forms are CNC'd, the forms have small holes drilled at the low points so the vacuum will pull the plastic in. There are limits as to how deep you can draw before the plastic becomes too thin. Since we are not terribly well set up the procedure looks like a Chinese fire drill. You have to be fast before the plastic starts to cool. Put the plastic in the frame before heating it. We use a 2" PVC pipe from the 40hp vacuum pump.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Limtech Industries, Inc. Lamello