Thoughts on a tunnel arch

2/20/17       
Mike Fuson

I'm going to be doing a tunnel arch in a doorway. Ive done laminated arches before but this one is going to be stile and rail profiled. Sort of a wainscoting look. My question is on how to run the stile profile on a piece that's done been laminated, and glued into the arch? Thanks.

2/20/17       #2: Thoughts on a tunnel arch ...
David R Sochar Member

Frame and panel is always best when it is - frame and panel. Whether you do the work as bent laminations or sawn from solid depends upon your preferences, abilities, the radius, and the needs of the job. I'd bend it all, if I could.

Profile your stiles and rails on the shaper with cutters oriented 90 degrees from the usual. What we call "stand up work" since the rails and stiles are run vertically rather than flat on the shaper.

The panel can be formed from thin laminations and then inserted and fastened into rabbets from the back. The cabinet panels in the photos below have moldings that were sawn from solid stock, then profiled as 'stand up work' and mitered together to retain the panels.

The panels were actually barrel built - narrow boards, each with a slight bevel to match the radius, hand planed a bit, and sanded. The raises were done as conventional along the straight sides, and as stand up on the ends. Just make or have cutters made to do either orientation.


View higher quality, full size image (1350 X 1800)


View higher quality, full size image (1800 X 1350)

2/21/17       #3: Thoughts on a tunnel arch ...
Read

David,

How do you orient a shaper cutter through 90 degrees, without having a horizontal spindle? Could you please send a photo of a work piece in the stand up mode?

Many thanks.

2/21/17       #4: Thoughts on a tunnel arch ...
TonyF

Mike Fuson:

Assuming that the tunnel is a radius, to profile the sticking on the curvature of a stile/rail, you would need to make a saddle for your shaper that corresponds to the concave curvature of your stile/rail. Align the cutter to the point where the stile/rail would pass through the cutter on the saddle and feed it through.

It would be best to laminate these stiles/rails, so that short grain is not an issue, as it would be if you were to bandsaw from thicker stock.

The stile/rail that is curved should be continuous when assembled/installed, i.e., the end of the curvature should abut the end of another curvature, so that the arc is continuous, and not have a straight rail/stile between the curvatures.

This is so that if a casing is a part of the project, the exposed offset of the casing will be a radius, rather than have flat sections in between. In a flat stile/rail of 3" in a 48" arc, the variation from the curvature would be about 3/64", which might look odd.

The bolection molding example that David shows in the photo would need only the groove or rabbet for the panel cut into the stile/rail, as the bolection molding would cover the edge of the stile/rail.

I hope I understood the question, and I hope this helps.
TonyF

2/24/17       #6: Thoughts on a tunnel arch ...
Mike Fuson

Thanks for the responses. David you do very nice work, I don't think I have the tooling to do it the way you do though.
Tony, your method is exactly on point with my thoughts. Thanks.

2/24/17       #7: Thoughts on a tunnel arch ...
pat gilbert

I'm sure you know but on the off chance you don't Decore makes curved doors.

2/26/17       #8: Thoughts on a tunnel arch ...
David R Sochar

My photos didn't quite convey what I think the OP is looking for. To do this - running 90 degrees from the 'usual' means having tooling made, or making your own. Not really a big deal. Curves can be run 'stand up' as I mentioned, or in a cradle in a lay down manner.

However, one must be careful with inside curves in a cradle for a tight radius, since the larger diameter cutters may re-mold the profile on exit. You'll know it if you see it. We like the lathe for tighter radii. It is great for making the tighter curves and then matching up to straights.

The tall cabinet has a slight outside curve on the face of the cornice, and two +/- 90 degree tight curves turned on the lathe, then straight returns on the sides.

The bonnet has an inside curve and two outside curves, all run flat on the shaper as one piece. We have the same knives made at 90 degrees so they can run a mold around something like a vertical cylinder also. Note the two minor curves level out as they turn the corner. Not doing this results in a 'developed' mold that can get very complex.

Now, when you have both - a vertical and horizontal curve - what we call a compound curve, then the party begins.....


View higher quality, full size image (750 X 1000)


View higher quality, full size image (1800 X 1350)


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Lamello