1/11/21       
Phil Member

Website: http://www.perriswoodworks.com

Hello,

I'm looking for some advice/input on the max span for some adjustable bookcase shelves. The design currently calls for 46" long shelves supported on either end by mortise mount pilasters/standards.

I'm wondering if I use 1 1/4" thick plywood with a hardword 1 1/2" nosing if that would be sufficient to prevent against sagging. Or should I suggest to add a middle vertical panel to reduce the span.

Thanks in advance.

1/11/21       #2: Max span for thick plywood shelves ...
DJS

You'll want to consider making a torsion box shelf for a span that size. 1/2" plywood top and bottom with 1/4" air gap in between.

1/12/21       #3: Max span for thick plywood shelves ...
Mark B Member

Sagulator would give you some honest feedback.

https://www.woodbin.com/calcs/sagulator/

1/12/21       #4: Max span for thick plywood shelves ...
David R Sochar Member

1. Sagulator - look to see the extent of the sag.
2. Torsion box - 1/8"or 1/4" faces on a egg crate core
3. Support the shelves in the center with a 5th point at the center back.

1/12/21       #5: Max span for thick plywood shelves ...
Phil Member

Thank you very much for the responses and for pointing me towards the "Sagulator." According to that, if I go with the 1.25" thick plywood and hardwood nosing I'll be within the allowable sag. I think I will add a 5th track in the center back as suggested to be on the safe side.

I have not built a torsion shelf before but it seems a like a great lightweight, strong alternative to what I was thinking.

1/13/21       #6: Max span for thick plywood shelves ...
mike berryman

I would think a 3/4 shelf tenoned into 3/4 solid front and back edge would be fine.

1/13/21       #7: Max span for thick plywood shelves ...
mike berryman

Let me add to my post that the edge would be 1 1/2 wide x 3/4 thick

1/15/21       #8: Max span for thick plywood shelves ...
Mark B

I have 3/4/ shelves with 1.5" hardwood edges that.were rebate/glue/screwed and plugged, many years ago (perhaps 25) that have clear and visible sag and they are only 36" long. Pillaster support holding books.

On a 4' shelf I'd personally shoot for half the Sagulators "acceptable" tolerance and make them finished all sides so they are flippable.

1/15/21       #9: Max span for thick plywood shelves ...
DJS

To understand the strength of a torsion box shelf, you simply need to let yourself imagine the following:

place a 3/4" thick piece of plywood across a pair of sawhorses 4' apart. Now set a 50lb box of nails in the middle, or a sack of concrete. The deflection would be considerable with or without a solid wood selfedge. Now try the same experiment with a hollow core door. Virtually no deflection, even when the door is comprised from basically 1/8" door skins and an interior made of cardboard. The strength is in the engineering. We build almost everything as torsion boxes; countertops, endpanels, floating shelves, adjustable shelves, etc.

1/16/21       #10: Max span for thick plywood shelves ...
Mark B Member

The torsion shelf makes all the sense in the world if your being paid for it. Its a lot more work than thicker ply or laminating two pieces of ply and applying a solid wood edge to the front and back faces. Dealing with all the edges/corners and cutting/assembling the core makes all the sense in the world if its necessary and billed in the job.

I'd have zero issue with an 1 1/2" (2 3/4" ply's) and hardwood edge. I'd guess the shrinkulator would have that one down in the 10-20% of acceptable range.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Limtech Industries, Inc. Lamello
    Today's Sponsors

    Become a Sponsor today!