Has anyone else experienced this on edgebanding?

7/5/22       
Justin  Member

I'm getting a ripple pattern on my parts and I'm having trouble figuring out why.
The long edges have a ripple pattern while the short edges do not.
There has been a black glaze applied that really shows the ripples as you can see.
I tried the edge tape on other parts and couldn't reproduce the issue.
My best guess from research is "milling waves".
Would this be because of the thickness of the part?
Any advise would be appreciated!


View higher quality, full size image (1253 X 943)

7/5/22       #2: Has anyone else experienced this on ...
RichC

Looks like a feed or pressure roller issue. How old are the rollers?

7/5/22       #3: Has anyone else experienced this on ...
Mark B Member

Whats the substrate? Have you been able to figure out if its telegraphing from the substrate or in the banding? Premill? No premill?

Looks clearly to be some sort of harmonic somewhere in the process either in milling the substrate and telegraphing through the banding or in the banding itself. You say it doesnt happen on short parts which narrows it down a bit.

7/5/22       #4: Has anyone else experienced this on ...
Justin  Member

@ RichC the rollers are good, thats what I had thought initially but the wavelength between the ripples is too narrow (in my opinion) to be one of the rollers.

@Mark B - it's particle core, we used the edge tape on other parts and couldn't reproduce the effect, so I figure that would eliminate the tape itself being the issue, it does get pre-milled.
It is a thicker substrate 1.25" vs the regular 62" thick substrate.

I'm kind of wondering if the milling feeds and speeds would need to be adjusted for thicker material but also, on the same material, the narrow ends didn't have this effect.
This really is a mystery to me!

7/5/22       #6: Has anyone else experienced this on ...
Mark B Member

Are you saying on the same part with a long edge and a short edge you only get the mill marks on the long edge with the same banding and operations?
To me the ripple is so precise it definitely speaks to a harmonic balance issue somewhere in the system and it would seem to most definitely be in the premill. We have a shaper in the shop that has a fussy spindle and when we edge material on that shaper and the spindle hasnt been clocked with an indicator, and using a helical insert head, we get the exact same result though its not banded. But all that is moot if your pre-milling other parts and they come out fine with the same banding.
That perfectly repeating pattern to me speaks to something harmonic in the process. Id be hard at the premill for either some out of balance, poorly set inserts, etc.. That pattern is so perfectly timed you know its some sort of a balance issue somewhere.
7/5/22       #7: Has anyone else experienced this on ...
Mark B Member

Run a test part without pre-mill and glaze it and see what happens. That would lock the pre-mill in/out immediately.

7/5/22       #8: Has anyone else experienced this on ...
RichC

When I zoom in on the picture, there is definitely different intensities to the black. A couple of places the intensity change is still very short. I think the thickness is causing some king of feed change yet. If it was the core and premillennialism, why would you get an intense black for 2" and then almost fade out towards the end of the board?

7/5/22       #9: Has anyone else experienced this on ...
RichC

*premilling

7/5/22       #10: Has anyone else experienced this on ...
Thomas Gardiner

Incorrect thickness adjustments on the pressure beam allowing the premill cutter to drift in an out with a set frequency. Just a guess.

7/5/22       #11: Has anyone else experienced this on ...
Leo G

I've seen this on pre-glued iron on edge banding. It comes that way from the factory and even a good sanding doesn't always get rid of it.

Test some raw edge banding that hasn't gone through the machine and see if the pattern is there.

7/6/22       #12: Has anyone else experienced this on ...
Justin  Member

@MarkB Yes, same part, same tape, same machine. Long edge got the ripple, short edge did not.
I will run some test parts soon and see what that looks like.

@RichC the part got glazed with a black glaze, that's where the black is coming from, they probably just wiped more of the glaze off of the ends.

7/6/22       #13: Has anyone else experienced this on ...
RichC

Well, applied glazing is a much different story.

7/6/22       #14: Has anyone else experienced this on ...
Not RichC

It was clearly stated it was an applied glaze.

7/6/22       #15: Has anyone else experienced this on ...
Mark B Member

Stange same banding same parts same everything and long edges have the marks and the short edges dont. Are all the parts cnc cut?

Keep posted. Be interesting to know what the final culprit is.

7/7/22       #16: Has anyone else experienced this on ...
Justin  Member

Yes all CNC cut, so there are many variables at play on this one.
I have yet to reproduce the problem, I will keep you guys posted though.

7/11/22       #17: Has anyone else experienced this on ...
Dave Edgerton  Member

Put some glaze on the un applied banding.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Limtech Industries, Inc. Lamello
    Today's Sponsors
    • NEMI
      Products For CNC Machines - Digitizers, Tool Setters, Vacuum Pods, Vacuum Cups, Vacuum Tables, Vacuum Chucks and Software
    • Southeast Tool, Inc.
      High Quality Tooling at Competitive Pricing
    • Cab Parts
      Pre-manufactured Components for Easy-to-Assemble Cabinet Boxes
    • Parts Cutter CNC
      CNC Cabinetry and Closet Parts
    • Western Dovetail
      Custom Made Dovetail Drawers
    • TradeJobPlacement.com
      Individualized Placement Services, Specializing in Millwork Design Engineers
    • iBiDMachinery
      The Nation's #1 Used Woodworking Marketplace - Buy and Sell Woodworking Equipment with iBiD!
    • 360 Degree Machinery
      Specializing in high end American, European, and select Import woodworking machines.
    • MARTIN Woodworking Machines Corp.
      Quality Woodworking Machinery Engineered and Manufactured in Germany
    • VortexTool Co. Inc.
      Manufacturers of Custom Cutting Tools, and Distributors of Major Cutting Tool Brands
    • RT Machine Co.
      Stocking Distributor of New and Used Woodworking Machinery
    • Centex Automation
      New and Used Machinery sales and service
    • TradeSoft
      Seamless Management Software to Improve Estimating, Job Costing, Scheduling, Purchasing, Shipping, and Shop Floor Data Collection

    Become a Sponsor today!