using a 1/2" solid carbide compression bit at 15,000 rpm and 600 ipm I can only cut 10 sheets of medium density melamine before my bit dulls. I also have tried a 3/8" at 15,000 and 600 ipm but get the same results. I increased the rpm to 18,000 and to a feed of 700 ipm but cannot tell it made any difference. What is the suggested rpm and ipm for cutting melamine and lam. particle boards?

3/20/15       #4: Melamine/Lam. cutting speed and fee ...
Gary B.

Randy,

I try to shoot for 0.023" chipload for melamine and laminate. For me, this means 16,000 rpm spindle speed, and 736 inches per minute for a 2 flute compression, or 1,104 for a 3 flute compression.

Your not that far off on the first numbers you listed. Have you looked at the collet care? Spindle runout? Not sure why they aren't lasting. I'm using Leuco brand, but Vortex, Onsrud, and Leitz all make good bits.

3/20/15       #5: Melamine/Lam. cutting speed and fee ...
Jay  Member

Website: http://www.hwccustomcabinetry.com

Try pushing it as hard as you can until you loose parts, have poor cut quality, or snap the tool. The bigger chip size, the cooler your tool stays, the longer it lasts. It is always a balancing act for these variables.
A LOT depends on your machine. How fast does it accelerate, de-accelerate, etc. When I ran Northwoods I could push a 3/8" 2 flute at 18k ~1200ipm new through 3/4" melamine, but kept it set at ~950 for my operators to make it easier. However 900ipm was all I could go on the Komo without breaking the tool.... I dunno why, it just did? My older, small CNT barely ramps up to 900ipm across the Y axis, I run a 3/8" 2 flute at 18K and still get good bit life even though its actual chip load (due to longer accl & decel times) is lower.
Don't be afraid to snap a tool a time or two to find the limits then operate just below them.

Hope that helps :-)

3/21/15       #6: Melamine/Lam. cutting speed and fee ...
Samuel  Member

You should try a 12.7mm Single Flute Compression Diamond Tipped from FS Tools made by FS Cruing, works great outlasts solid carbide bits we have. FS Cruing has many other Diamond tipped Router bits for the woodworking industry you should check it out.

3/22/15       #7: Melamine/Lam. cutting speed and fee ...
Larry

We are running 3/8" 2 flute compression Onsrud Marton bits (coated) We will get 60 sheets of melamine and another 30 sheets of MDF or particle board. Running a Komo @600",16K. When the bit is new we will push it a bit faster, 700". It is running cool enough you can take hold of it right after it stops. HPL is hard on bits we will only get about 25-30 sheets on it. I like to have a very clean cut, no crushing of the melamine face or burring of the HPL. The problem with the diamond bits is they are usually single flute, meaning your feed rate has to be slowed a lot.

3/22/15       #8: Melamine/Lam. cutting speed and fee ...
Samuel  Member

Larry-- Yes your right because of the single flute we run it slower but, you can get a two flute of three flute diamond bit if you wanted to. We are using a single flute just because thats what we have usually used but we would like to look into the two flute or three flute but they cost more, but at the same time they do last a while.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Onsrud Cutter Vortex Tool Company T-Tool USA Limtech Industries, Inc.