Subject: Re: Major problem.....cherry and gray

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Major problem.....cherry and gray

7/1/15       
Justin h

Have a huge job ready to be installed and can't get the color right. Customer initially wanted cherry cabinets to match durasupremes morell on cherry. Then after picking floor out they wanted it to be more gray rather than the brownish gray. I talked them into using birch....then my sales rep talked me back into cherry and said won't be a problem getting it gray.....well i put my trust in him as I didn't have time to play around with colors....

Well guess what....not having any luck. Can't kill the red or it turns blue. Working on a possible dye next. Any one else come across this??

7/1/15       #2: Major problem.....cherry and gray ...
Kevin

i would be calling my sales rep who said it wouldnt be a problem getting it grey and let him make up a stain formula since its no problem. Other than that, you have a tough one here buddy. Try using blue and yellow dye with mixed into some acetone with white vinyl basecoat.

This is where i would begin the matching process :

Acetone : 400 grams
(S61 y504) Yellow dye concentrate : 1 gram
(S61 L505) Blue dye concentrate : 1 gram +/-
(S61 B500) Black dye concentrate : .4 gram
(P63 W9) White vinyl basecoat : 5-10 grams.

7/1/15       #3: Major problem.....cherry and gray ...
Robert

Website: http://www.threenailswoodworking.com

You are not going to get there in one step stain process. Just not going to happen.

It might take a stain, glaze and toner to get that all the way out. Start more white than you have to. Sherwin Williams has a great white stain that is heavy on pigment. Leave it on very heavy. Then build off that. We usually accomplish it with a glaze but a toner, or a glaze/toner combo would work.

Good luck. Robert

7/1/15       #4: Major problem.....cherry and gray ...
Robert Member

Have you considered a light bleaching using the Wood-Kote bleach. It can be sprayed on,it wont leave a crusty mess like some bleaches do and it wont burn the wood if applied correctly.

One of those Plastic pesticide sprayers work quite well and if you get one with an adjustable nozzle you can get a one foot wide spray pattern.

Rather than try a whole bunch of staining and glazing and toning processes try bleaching a piece of Cherry. It might make your whole coloring process much easier to deal with. You may get to the desired color quicker too.

7/2/15       #5: Major problem.....cherry and gray ...
Pete Anderson

Website: http://petesfloors.wordpress.com

If you are going to use a garden sprayer you can save time by drilling a hole for a tubeless tire stem so you can fill with compressed air. Don't fill more than 30 psi.

7/2/15       #6: Major problem.....cherry and gray ...
afinisher

I'm sure Robert knows this but for general info - If you spray the 2 part bleach, please be extra careful not to breathe any amount of it or allow exposure to skin or eyes. It is very caustic. If you use a mask make sure the cartridges are rated for that material

7/2/15       #7: Major problem.....cherry and gray ...
Robert Member

Good of you to post the safety precautions afinisher, they completely slipped my mind.Thanks for the correction.

7/3/15       #8: Major problem.....cherry and gray ...
Gene Wengert-WoodDoc

Cherry wood is very sensitive to acidity, forming a blood red color if exposed to caustic materials...that is, if the finish is above pH 7.0. Likewise, stronger acids result in red colors. So, the finish material needs to be neutral.

Second point is that wood bleach (oxalic acid) is probably a better material than chlorine bleach. Safer too.

The difficulty with any bleach is neutralizing it before proceeding with the next step. Drying alone is not sufficient. The bleach should be washed off, in most cases.

7/18/15       #9: Major problem.....cherry and gray ...
Matt

Blue color will not kill the red. It will just turn it purple.

See if your tint specialist can make you a green dye. Spray that on your wood, let it dry for a minute, and then apply the gray wiping stain.

The green dye will tend to kill the red in the cherry. It will be 'darker' than it was to begin with.

If you must get even more gray, use some gray pigmented CV mixed in with your clear to make something of a pickling-topcoat effect. This will washout the grain a little but also impart a lot of the gray you are looking for, while still having at least some grain underneath.

For future jobs, I would recommend you use maple, rather than birch or cherry. Cherry, for obvious reasons, but even the birch can be rather yellow, making the gray stain more difficult.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)