Subject: Re: Stripes in Finish

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Stripes in Finish

5/24/18       
scott

Just finished spraying ML Campbell Stealth with a Kremlin MVX Gun, MX 14 cap and 09-094 tip. fluid pressure 30lb. air pressure 10 lb. CV 275 voc with 5% catalized, 3% retarder, 10% reducer sprayed 8" from surface with a 50% overlap. Panel is coated wet but when dries appears to have stripes. I have upped both fluid and air pressures and eliminated reducer with same effects. Any ideas or solutions as to what I'm doing wrong, had this happen with clear CV awhile back but can't remember how i fixed it. Have sprayed for the last 2 years this way with no problems. Thanks for input.

5/24/18       #2: Stripes in Finish ...
Hen Bob Member

Stealth has a 10% catalyst ratio..

5/24/18       #3: Stripes in Finish ...
rich c.

8" is pretty close, move the gun back.

5/24/18       #4: Stripes in Finish ...
John Member

Have you shot some burst patterns to see if it's uniform.

John

5/25/18       #5: Stripes in Finish ...
scott

Spraying in Southern Cal. so Stealth is 275 VOC. and uses new 5% catalyst mix. has been like this for several years. Getting new tip for gun today and will try some tests with gun farther from surface. thanks for input.

5/25/18       #6: Stripes in Finish ...
Scott Gibson

Not sure about Stealth 275 but we spray regular Stealth and reduce it with their Flow Enhancer instead of lacquer thinner. Seems to flow out nicely. Also, we spray it pretty heavy.

5/25/18       #7: Stripes in Finish ...
DannyB

Ignoring any tip issues here (which i bet is the likely cause):

Stealth is regularly very high viscosity (70 seconds ford #4) and has to be thinned. It's about 250 CPS.

Stealth 275/Sl is currently very low viscosity (10-15 seconds ford #4). It's about 20-40 CPS (so 5-10x less viscous).

I thought Stealth 275 was reformulated a bit into Stealth SL (stealth 275 used to be thicker) , and this was done before changing the label to say "Stealth SL".
Now i can't remember if they reformulated stealth SL or just renamed it.
If i'm remembering right, one thing that happened was that it got thinner than it used to be.

I mention all this because as you can imagine, Stealth definitely requires thinning. Stealth SL (these days) shouldn't require thinning at all, and is very thin already. It's thinner than a lot of spray stains. For reference, the viscosity of the microton spray dyes is 8-9 seconds.

You also definitely can't easily apply things that work for Stealth to Stealth 275/SL.

Here, i definitely would actually stop thinning it, unless you are doing it to have it flow better on hot days or whatever.

(I only know all the above the hard way -
I went from regular to 275, and after frustrating myself to death one day, i realized i was using way too large a tip)

5/25/18       #8: Stripes in Finish ...
scott

OK so got a new 09-094 tip from kremlin as per their suggestion which is what we have used for over 10 years. using the Stealth 275 voc for california, i catalyzed 5% with appropiate catalyst, reduced 20% with care extender and 5% retarder with 35lbs. of fluid and had to go 20lbs. of air to remove tails and sprayed wet coat. Same problem. Makes me want to go back to pre cat Magna max where the only problem was drying time. Still up for suggestions.

5/27/18       #9: Stripes in Finish ...
rich c.

Did you do a series of fan pattern tests by just pulling the trigger into a piece of brown paper or scrap dark hardboard? See if the fan pattern is even at the distance away from the stock. Pull the gun back further, closer, more air, etc. Then you know more knowledge about the pattern. Don't spray a big panel expecting to analyze the fan pattern.

5/28/18       #10: Stripes in Finish ...
John Member

Have you talked about this with ML Campbell?

If the spray pattern is indeed OK then it seems like the finish is setting up too quickly, so the next pass doesn't flow into the one before it completely. If so, adding more retarder would be the right move.

John

5/29/18       #11: Stripes in Finish ...
Shane

tip is too small for that C.V.
Keep the same mix you have. Overlap passes as you have been doing.
I guarantee if you move the gun to 10-12" from surface and change your tip to 12-174 youll be getting a much nicer finish. You may have to move a touch faster but you'll be putting down the correct wet coat and the right wet millage at that rate for bigger panels..... shooting with an 09 would be like being stuck in second gear instead of overdrive.....Get your material down faster and the right thickness will help it all have a moment to flow out and do it's thing...

6/4/18       #12: Stripes in Finish ...
scott

OK I'm back with results, after trying different mixes and fluid and air settings we were unable to get satisfactory results and my rep was to contact ML Campbell. We decided to switch to Magna max to expedite and try and get this job finished while waiting for answer from ML Campbell. So after spraying i now have encountered a million micro dots that feel smooth but are visible.
Shane i will order the other kremlin tip12-174 to try with the CV.
Anybody have a fix for the Magna max - no stripes but now micro holes???

6/5/18       #13: Stripes in Finish ...
scott

Back again after another day of trials and info from ML Campbell. Not enough retarder, not wet enough on coverage!!

So we put 5% and gave it a good wet coat-WRONG.
10% - WRONG
15% -WRONG
Said maybe it was to hot 85'-90', ok i will come back and spray in morning.

I'm back at 4;30 in am its 60', the magna max with 15% retarder, feels perfect and sprayed a nice wet coat with a 50% overlap. Nope still getting micro dots.

I've never used 15% retarder , maybe 5% max. I'm still looking for answers.

6/5/18       #14: Stripes in Finish ...
John Member

I had a lot of little bubbles with Target Coatings EM9300. Target said I was using too small a N/N on my HVLP gun, even though the viscosity said otherwise. I upsized the N/N to what they recommended. Actually, it was the minimum the recommended, I could have gone even larger. There were fewer bubbles, but not perfect. I moved on to a different product rather than try an even larger N/N, but the point is, this might be the right direction to resolve your problems. Worth a try if you have a larger tip to try.

Have you tried spraying either of these products with a different gun type?

John

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)