Subject: Re: how to close the pore ?

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

how to close the pore ?

5/3/20       
mauricio poli Member

Hi everybody!
We have lot of work trying to speed up the finishing process of solid pine coffe tables.
In some pieces, we found open pores only after stain and first pu sealer coat.
Then we use a medical syringe to fill the pore with sealer, and have to wait several hours to sand it.
After we sand the bare wood, we are using filler, but those defects are difficult to see.
What can we do to avoid this, or to easily close this defect?
Thanks a lot.


View higher quality, full size image (3120 X 4160)

5/4/20       #2: how to close the pore ? ...
Dan Cook

You can use a paste filler before finish coat which fills all the pores, but it is not quick. You basically cover the entire surface, let it dry and then sand to smooth before staining and finishing, but it eliminates the open pore situation. It is not quick, but permanently fixes the problem instead of going back and trying to fill open pores which if you are using catalyzed finishes that don't rewet are probably showing through the next coat.

5/4/20       #3: how to close the pore ? ...
rich c.

Looks to me like a bad glue seam instead of wood pores. More careful handling and a better job of jointing the edge should eliminate a lot of that. I preferred Famowood solvent based for tiny imperfections.

5/5/20       #4: how to close the pore ? ...
mauricio poli Member

Thank you very much Dan and Rich!
Dan, do you believe it I use a water based filler between the coats it will help?
Rich, We are using automotive filler, do you believe solvent famowood is better for the wood? I am going to check how our people are glueing th pieces.
Thanks

5/5/20       #5: how to close the pore ? ...
GaryE

Website: http://www.wurthlac.com

As said above, best practice for a full fill is to use a paste wood grain-filler. There are a number of these on the market. The one I am familiar with is either brushed or sprayed (reduced) to the raw wood, and wiped into the grain almost similar to wiping a stain. roughly 4 hr dry time, then sand back and seal. They can usually be tinted also, but once dry, they are clear.

I've attached a link to the product I'm familiar with below.

-Gary

ML Campbell FD Wood Filler Paste

5/5/20       #6: how to close the pore ? ...
mauricio poli Member

Thanks a lot Gary!

5/7/20       #7: how to close the pore ? ...
duster

Gary - what do you use to thin the MLC paste filler?

5/7/20       #8: how to close the pore ? ...
rich c.

So with all the wood grain fillers being mentioned and suggested, you guys routinely fill pine? It would be a task to fill that whole pine table top just to fill a gap at that seam.

5/7/20       #9: how to close the pore ? ...
DannyB

Yeah, i think i agree with where Rich is going.

As a production process for filling pine that will have a bunch of deeper seam gaps, etc, i would probably be squeeging epoxy over the entire thing or something that will fill it all in one pass.

If it was a real production process, i'd use uv cure epoxy so i could recycle the extra, but this doesn't sound high volume enough.

5/9/20       #10: how to close the pore ? ...
mauricio poli Member

Hello everybody!
Let me tell you how we solve this pore problem.
First of all we check the glueing, and get better, fewer pores.
After we put 2 heavy pu sealer coats wet on wet, sanding 320 and repeat another 2 heavy coates.
In the last sanding, there were some pores yet....
Then we put color on an automotive poliester filler, and very carefully we fill the tiny pores with it.
After the final coat, it is very good no more pores.
Thanks everybody!

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!