Total Finishing Supplies

Professional Finishing

You are not logged in. [ Login ] Why log in
(NOTE: Login is not required to post)

Post a Response
The staff at WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at any WOODWEB Forum. Participants should undertake the use of machinery, materials and methods discussed after considerate evaluation, and at their own risk.
Your Name:
Your Website:
Email Address:
Subject: Re: Water based poly over oil based

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Water based poly over oil based

3/8/21       
Phil Member

Hi ,

Does anyone have experience doing water-based polyurethane over oil-based polyurethane? I like the amber of the oil based but it takes so long to dry I am getting some dust nibs in it. Was wondering if I could use the oil based to get the color, sand out any nibs, then top coat with a faster drying water based poly. If so , how long should I wait for the oil based to cure? Thank you!

3/8/21       #2: Water based poly over oil based ...
rich c

You don't mention any product names, but in most cases the water based won't bond.

3/8/21       #3: Water based poly over oil based ...
Phil Member

Sorry, the specific products would by Old Masters Oil Based Poly followed by Old Masters Armor

3/9/21       #4: Water based poly over oil based ...
Adam

It's been a common issue for a long time. The wood finishing gods gave us Zinsser Sealcoat. It's dewaxed shellac. Amber, decent sanding sealer, pops the grain better than oil. 100% compatible with wb. What's not to like?

3/9/21       #5: Water based poly over oil based ...
Phil Member

Thanks Adam! Could I use SealCoat over an oil based stain , then go with a water based top coat.

3/9/21       #6: Water based poly over oil based ...
Phil Member

Also, on the Masters Armor (wb) can it says not to use over anything containing stearates? Do you happen to know if SealCoat contains stearates?

3/9/21       #7: Water based poly over oil based ...
MarkB Member

While the can is the can, most modern waterbournes dont suffer the issues of adhesion with stearates that happen years ago. Good wipe down with DNA or even water and there will likely never be an issue. But always good to follow the can.

In our experience is pretty tough to come across something you cant run WB over. While the WB wont cut into any finish (though Target says they have a burn in WB) with a good scuff/scratch my opinion is your pretty safe over most anything.

If your looking for a bit of the amber in a single application and you have access you may look into MLCampbell Magnamax H2O. It aims for that amber cast.

Im not a fan of shellac unless its necessary but its a decent alternative.

3/9/21       #8: Water based poly over oil based ...
John Member

Sealcoat shellac, as mentioned, would be a better alternative than OB poly first. But there are other ways to get the amber look of OB poly with a WB product. First, General Finishes EnduroVar has an amber tint built in. Target Coatings EM-2000 is even more amber because it's actually an OB varnish emulsion. MInWax makes a hybrid product as well.

Alternatively, you can dye the substrate or add dye directly to your WB topcoat to give you an amber tone. There are lots of ways to go about it. Putting WB over OB poly, however, is not a route I would take.

Be aware that some WB products craze when applied over a heavy coat of Sealcoat. Test.

John

3/9/21       #9: Water based poly over oil based ...
Phil Member

Really appreciate the feedback. On a related note, what would you recommend using as a stain if I use a WB product like Target EM 2000 or EnduroVar. I'm most comfortable with oil based stains (including gel stains) but again not sure of the compatibility between those and a WB topcoat.

3/9/21       #10: Water based poly over oil based ...
John Member

WB is best under WB topcoats, but I've never had any problems using oil based ones IF I wait at least 72 hours for it to dry. Not very good for a production operation to be sure. Products like SW's BAC Wiping Stains, however, can be top coated in only a few hours. In both cases, I spray a light coat of Sealcoat shellac first.

More recently, I've found if I add some of BM's Extender to a WB stain I have a lot more working time with it and it behaves more like an oil based product.

John

3/11/21       #11: Water based poly over oil based ...
MarkB Member

We spray almost daily over BAC, Ml Cambell spray and wipe (Woodsong II), etc. with no hours of wait time. Its not uncommon to have a remake of a part that will get sprayed in less than an hour and never had any issues whatsoever. I have never waited hours/days to clear over any stain though we dont use home center/minwax stains but I wouldnt wait with those either.

3/11/21       #12: Water based poly over oil based ...
Adam

MLC Woodsong is a very high quality stain. It’s got some fast evaporating acetone like solvent that make it dry quickly. Not surprising that it doesn’t bother wb topcoats.

We used it exclusively when we did solvent. It’s our go to under web when some architect specs Minwax golden oak.

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!