Subject: Re: lacquer finish 6 months old is peeling and coming off

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

lacquer finish 6 months old is peeling and coming off

4/11/21       
Steve Member

I used pre cat lacquer to finish a set of cabinets about 10 months ago. 3-4 months later the finish was peeling and coming off in spots. only around the sink and DW area. Refinished those with a new can of lacquer 6 months ago and now it is coming off again. I used a sand and sealer first (no stain,natural oak) and 4-5 coats of lacquer , just like always. No complaints before when I used Gemini but seems like everything I finished with a different manufacture I am having trouble with. Any help on why this is happening would be appreciated. The laq. I used was sold by a cab. supplier. When i used it the manufacterer said it was still within exp.date. I am going to switch to Gemini CV, what should I know about CV?

4/11/21       #2: lacquer finish 6 months old is peel ...
rich c

Explain the "sand and sealer" and if you sanded that before top coating. Most pre cat directions will say to use vinyl sealer or just seal with the first coat of pre cat. In my experience, pre cat and lacquer will never last around heat and high moisture. I've never had it peel off, but some crazing and cloudiness. Luckily it was on my kitchen before I started doing cabinets in my business.

4/12/21       #3: lacquer finish 6 months old is peel ...
Steve Member

Thanks Rich, I put 2 coats of vinyl sealer. I sanded after 1 coat but not after no. 2. I then applied 4 coats of pre cat lacquer. This was after I sanded the doors. They were finished natural.

4/12/21       #4: lacquer finish 6 months old is peel ...
Tom Gafgen

Six coats of precat lacquer most likely exceeded the recommended dry film build which can cause adhesion issues .

4/12/21       #5: lacquer finish 6 months old is peel ...
rich c

Tom's right. They have very strict maximum thickness rules. I believe most say 2 coats max unless you really lay it on thin.

4/13/21       #6: lacquer finish 6 months old is peel ...
Mark Member

I switched to CV for this very reason. Biggest difference with CV is the time you have to work with after you catalyze it. I mix in small batches and use a hopper based airless sprayer with 15' hose. I do like the finish better, seems to be more durable. No issues with areas of high moisture either.

4/13/21       #7: lacquer finish 6 months old is peel ...
Adam

You didn’t sand between the vinyl sealer and precat laquer. The laquer is probably too thick and you encouraged it to not bond to the sealer.

4/15/21       #8: lacquer finish 6 months old is peel ...
Steve

Hey everyone I appreciate all the feedback on my problem. I have always put 3-4 coats of lacquer on the base cabinets, I figured more was better protection where it was needed but I guess not when it comes to number of coats. I am thinking about switching to CV.

4/17/21       #9: lacquer finish 6 months old is peel ...
cabinetmaker

The vinyl sealer has a top coat window. I’m thinking not only do you have a mil thickness as too much problem,you also created a bind problem with two coats of vinyl.

We switched to cv ml Campbell Crystal or SW kemvar with stellar results spraying railings and wall panel pckgs for schools not to mention kitchens.

We do use the sanding sealer as it helps with a gumming up issue.

We sand with 320 after the first coat snd hit it with 2 coats after with 2 oz of flow enhancer per gallon after 10% catalyzinv waiting for a burn in of the catalyst to coating.

It’s pretty forgiving snd straight forward. Great results and great durability. Gemini. Is a decent product always has good luck We use ml Campbell as it comes in with lots of panels melamine or quartz from the sand supplier

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!