Subject: Re: Wood Countertop Finish Over CV-Based Stain\Glaze

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Wood Countertop Finish Over CV-Based Stain\Glaze

9/15/21       
Vincent Musser Member

Building maple butcher block tops for a client. They like a medium stain color that I achieved using the product that I typically use under Sherwin Williams CV (dye with lots of wash coats and glaze to arrive at desired color).

I am reading that CV is a less-than-ideal finish for a kitchen counter top. This top will not be cut directly on, but will get heavy everyday use.

Does anyone know of a good counter top finish that can go over a catalyzed stain sequence with good adhesion and have a sheen similar to dull rubbed?

9/15/21       #2: Wood Countertop Finish Over CV-Base ...
Mastercabman

Never heard of a "catalyzed" stain before but most people use 2K poly as a finish for counter top

9/16/21       #3: Wood Countertop Finish Over CV-Base ...
shenendoah

Vincent, rule of thumb:
One's washcoat coating should be of the same variety as one's topcoat. I.E. If the washcoat is cv based - sealer or topcoat, then your topcoat should not be 2P k urethane or polyester. Having started with cv wash, you shouldn't "upgrade" to strengthen. Huge potential for coating failure.
Especially with multiple washcoats locking in, I assume, multiple glazes. Which in itself can lead to potential film failure especially on a well used table top.
So if one were to want a 2P k urethane or polyester topcoat, one would need to use an isolante/barrier coat(s) between glazes, if the glazes were petroleum based.

9/16/21       #4: Wood Countertop Finish Over CV-Base ...
Mastercabman

Somehow I missed your first paragraph

So like Shenendoah said,you should stick within the system
I suggested 2K poly because it's what most wood countertops fabricators uses for their finish
So you might have to get stain and whatever else you need to be compatible with the 2K poly

9/17/21       #5: Wood Countertop Finish Over CV-Base ...
Vince Member

Thanks for the info so far, guys.

I use SW products, and went ahead and looked up their 2k poly. It's called procraft 9300 polyurethane clear coat.

I had a couple questions about it's use (mainly spray and cure temps), and talked with Sherwin Williams main tech support line.

The guy told me that they cannot recommend this, or any of their products as a food safe kitchen countertop finish. He told me to look into a pourable bar top epoxy, which I know I don't want to use!

My client has already agreed not to cut directly on the tops.. but now I feel put on the line as to whether or not to open the can of worms and tell them it's actually not food safe rated..

I know I won't be able to get as good a stain/finish using Waterlox or epoxy..

Frustrating!

Guess that's why they call it work.

9/18/21       #6: Wood Countertop Finish Over CV-Base ...
Pete Anderson

Website: http://petesfloors.wordpress.com

I have used conversion varnish as a sealer, usually two coats, then moisture cure poly-urethane as finish, either satin or gloss. Harco Coatings makes MC POLY that has a tile like glaze. I've had it on our maple counter top for years.

9/18/21       #7: Wood Countertop Finish Over CV-Base ...
Vince Member

Pete,

That sounds like the best solution to me so far. I am having trouble finding a gallon or quart of moisture cure in dull rubbed, or even satin, though.

I am only seeing it on gloss.

9/18/21       #8: Wood Countertop Finish Over CV-Base ...
Vincent Musser Member

What about putting plain old satin minwax poly over 320 grit-sanded CV?

9/18/21       #9: Wood Countertop Finish Over CV-Base ...
Vince Member

Test board coated.

It's a sample board I made a couple weeks ago with a stain sequence and CV.

I coated the poly over: no prep, 220 grit sanded, and 320 grit sanded.


View higher quality, full size image (4032 X 3024)

9/18/21       #10: Wood Countertop Finish Over CV-Base ...
Pete

Gloss MC poly can be rubbed out with fine steel wool.

9/18/21       #11: Wood Countertop Finish Over CV-Base ...
Vince Member

Oh nice.

I didn't think of that.. been spraying CV so long.

So I'm guessing the mc poly has better adhesive qualities than some old minwax?

9/20/21       #12: Wood Countertop Finish Over CV-Base ...
Vince Member

Sample board pic below.

The area with no sanding did not offer any adhesion.

The CV sanded with 220 grit allowed the poly to adhere 100% when tested with tape as well as scraping.

I did not bother checking the 150 grit.


View higher quality, full size image (4032 X 3024)

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!