Subject: Re: Conversion varnish specks

Message:

(read message guidelines).
Note: Do not use the below fields to advertise your business - only for links related to the discussion.
Thread Related Link URL:
Thread Related Link Title:
  To "point" to an image (picture) from another website, provide the URL (Web Address) of the file ( include ONE reference to http:// )
Thread Related Image URL:

Date of your Birth:

Upload a Thread Related File:
File Types: Image (gif-jpg-png-bmp), PDF, Sketchup, Video (mov avi wmv mpeg mpg mp4 ogg). (Image Upload Tips)

I have read the Site User Agreement and agree with the Terms

  <= Check to receive e-mail notification of responses

Message Thread:

Conversion varnish specks

2/17/22       
Nathan Grabowski Member

We have sprayed atleast 100 gallons of sherwin Williams kemvar plus. Mostly white, but quite a few other colors as well. Today for the first time everytime I spray there are fine specks showing up in the finish. The finish is spraying fine and laying nicely but then as it dries it shows more of these randomly distributed things that almost look like grains of sand. If you squeeze one they are soft and will basically dissolve between your fingers but they will harden when left on the surface. I have sprayed 3 different cvs I had in the shop and it is doing it on all and all had sprayed fine previously. I completely tore down and cleaned the gun I was using and tried a second gun and tried prefiltering in addition to the filter on the gun. The last thing I tried was I had a little catalyst left in an old bottle but using it didn’t seem to matter. The only thing I haven’t tried is changing to a new thing of reducer, which is the recommended r7 k310. If anyone has any ideas I would greatly appreciate it. Thank you

2/17/22       #2: Conversion varnish specks ...
Leo G Member

Replace your fluid line.

2/17/22       #3: Conversion varnish specks ...
Nathan Grabowski Member

We are spraying with an a Apollo turbine and cup gun, so there is no fluid line to clean unfortunately. I spoke with a sw rep and his guess is that it is actually micro bubbles showing as small nibs. Anyone else experienced that?

2/18/22       #4: Conversion varnish specks ...
Karla Gossling

Could it be the flattening agent not completely agitated and dissolved?

2/18/22       #5: Conversion varnish specks ...
Roy Cameron

Try cleaning your filters on the turbine. Maybe some dust got into the turbine as well.

2/19/22       #6: Conversion varnish specks ...
RichC

Do you strain the finish when pouring into the gun?

2/20/22       #7: Conversion varnish specks ...
Nathan Grabowski Member

So here’s an update and I am just as lost if not more at this point. To answer some questions, yes I cleaned and replaced turbine filters, on two separate machines. I predilter everything through a conical strainer before it goes in the gun. I even had a can of Kem Aqua plus laying around and sprayed that and had the same results, so no shared materials in that situation. So I figured it had to be something with the turbine system or hose. I hooked the gun up to my compressor and have the same specks spraying out. So basically I am rethinking my entire existence at this point

2/20/22       #8: Conversion varnish specks ...
Nathan Grabowski Member

So I realized I was spraying the same cup of finish I had been working with last night. I strained it out of the cup and it was full of junk. So I then strained from the mixing cup it had come from originally and it was clean.
So clearly I am getting contaminated air somehow. Going to do a few more tests with compressed air now and see what happens

2/20/22       #9: Conversion varnish specks ...
shant K avedisian

we use chemcraft product by Axnobil we normaiily mix 8.oz of acetone and 8.oz of MAK and 13.oz of catalyst and the finish is beautiful but this formula has to be all chemcraft its the best finishing product out there hands down

2/20/22       #10: Conversion varnish specks ...
Mastercabman

How's the weather where you are?
Is it possible that your turbine is picking up moisture?
I would go buy a cheap gravity feed spray gun and do a test
If it doesn't happen then it's your equipment
If it does happen then it's the product/environment condition

2/20/22       #11: Conversion varnish specks ...
Nathan Grabowski Member

So I realized I was spraying the same cup of finish I had been working with last night. I strained it out of the cup and it was full of junk. So I then strained from the mixing cup it had come from originally and it was clean.
So clearly I am getting contaminated air somehow. Going to do a few more tests with compressed air now and see what happens

2/21/22       #12: Conversion varnish specks ...
Nathan Grabowski Member

Humidity in the shop is about 25%.
Cleaned the entire shop, set up a gun with the compressor and a dryer/filter regulator on it. Same results. Sprayed a piece outside and had basically the same result. After doing testing I have found what almost looks like small bits of silica in the spray cup. Can’t ever remember seeing that before but ask probably never studied it that closely. Sw rep is doing testing with our materials today, so I’ll see what he says and then go from there I guess.

2/21/22       #13: Conversion varnish specks ...
Leo G Member

Their material will be perfect.

of course.

2/24/22       #14: Conversion varnish specks ...
Dan

This is something I’ve heard more than I actually have experience with…. But if it’s a good chance your air is contaminated as in something in your tank or if it’s a rotary screw you are getting oil into your system. With a piston it’s not that much of a problem but could still be getting something in. I would get some good filters in your air line and try that.

2/24/22       #15: Conversion varnish specks ...
Nathan Grabowski Member

So as of right now it looks like it was a product issue. I am spraying their next generation of kemvar today and it is spraying nicely with no specks or nibs. I do give sw and their rep credit for not just brushing me off on this and taking the time to actual look into it and get me set up with a product that is working well.

2/26/22       #16: Conversion varnish specks ...
Hakam G

Simple ..... thin your material down and add little bit of retarder , what's happening is your gun has open fan all the way and breaking uour paint ,conversion varnish is different than 2k finishes it likes to be heavy so ehat i do is i spray first cote and let it sit fir 3 minutes then i hammer second cote on and sometimes i spray 3 ...... you will notice that the more you spray it wet on wet the more it flows and all these pinholes will disappear , also depends on your spray gun i hold it back about 8 inches away from surface

 

Buy & Sell Exchanges | Forums | Galleries | Site Map

FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!