11/17/15       
Louis Brandt

We use MDF for painted slab doors and cabinets. Our finisher insists on sanding the faces of parts to 320g prior to finishing. The edges are banded with maple veneer. We are spraying opaque catalyzed conversion varnish from ML Campbell. My hunch is that the parts only need to be sanded to 150 prior to primer. We're doing 120g, 150g, 180g, 220g, 320g. All with a Festool orbital. Seems excessive to me. What do you think?

11/17/15       #2: Sanding MDF for paint ...
Kevin

sanding that high will cause adhesion issues. your instincts are correct. we sand to 150 before primer to allow the primer to bite real good.
not only are you wasting time and material, you are actually creating a surface that is to polished to accept a coat.

11/17/15       #3: Sanding MDF for paint ...
Louis Brandt

Well, that explains why my finisher doesn't like blue tape; he says it's too sticky an pulls the finish off.

11/17/15       #4: Sanding MDF for paint ...
JeffD

Yup, Kevin is right, you can find the specs for ML products online, print them out and hand them to your finisher. IIRC 150 is about the highest you should sand to, I usually do 120 grit, 2 coats of Clawlock, then 2 coats of Resistant for what I consider a very nice finish.

I wouldn't use blue tape either until it's dried at least a couple days. It shouldn't lift the finish but it will leave a discoloration on the surface covered if used to soon….I learned that one the hard way!

good luck,
JeffD

11/17/15       #5: Sanding MDF for paint ...
Adam West  Member

Website: http://www.surfprepsanding.com

320 on the compressed face of MDF is not necessary at all. I do often use 320 for the edges and routed profiles and it works wonders for smoothing the texture so the MDF won't suck in so much finish.

150 grit on the face is too rough. Too coarse a grit will pull up the fibers that you want to leave in place in the tight surface. 220 is a better choice. You don't want to grind off much of any material. Just remove the scratch pattern from the mill that made it and get rid of handling marks.

11/18/15       #6: Sanding MDF for paint ...
Louis Brandt

I just called tech support at ML Campbell, and they recommend 320g for the faces of MDF, 400g for the edges. Not what I wanted to hear.

11/18/15       #7: Sanding MDF for paint ...
Rick Mosher

Do your own adhesion test and find out for yourself what works and what doesn't.

Adhesion testing

11/18/15       #8: Sanding MDF for paint ...
Joe Member

My ML Campbell finishing rep had recommended this some time back. I use the Agualente waterborne. Sanding at the 320 and 400 end grain, has never failed me.

11/18/15       #9: Sanding MDF for paint ...
Rick Mosher  Member

Website: profinisher.blogspot.com/

A WB product would be different than a solvent based one. The water will raise the grain a little promoting adhesion better.

11/18/15       #10: Sanding MDF for paint ...
Kevin

i have to admit i am absolutely shocked. You mean to tell me that ive been sanding ALLL my mdf wrong this whole time? I mean, i couldnt even begin to count how many miles of mdf panels i run thru my heeseman sander with a 150 grit belt every day right before they hit my cefla to be primed, then back to the heeseman for scuff then back to cefla for paint.

Not sure what works for you, but i like conversion varnish that adheres so well it takes a jack hammer to chip it. And i get that from 150.

If you take the advice of a professional finisher, you get good finishes. Take the advice of a sanding supply salesperson, you buy more sandpaper.

11/18/15       #11: Sanding MDF for paint ...
Kevin

FYI:

i just pulled this off the ML Campbell website. This is in the data sheet for clawlock primer :

Surface Preparation
New Work:
Remove any dirt, grease, glue or other construction contaminants and sand wood as
required. When using high solids coatings on wood, it is important that the wood retains a
profile after sanding for the coating to lock onto. High solids coating like Clawlock require a
slight profile left on the wood after sanding. For best adhesion, finish sanding on wood,
should be done using a maximum of 150 grit paper. Always be sure that sanding belts and
sand paper used are not worn, as worn sanding materials tend to polish the wood.

---- " For best adhesion, finish sanding on wood,
should be done using a maximum of 150 grit paper"

11/18/15       #12: Sanding MDF for paint ...
Kevin

heres the data page

ML Campbell Clawlock Primer

11/18/15       #13: Sanding MDF for paint ...
Louis Brandt

Yeah, I saw that on the website. They also had an additional section about MDF:

Remove any dirt, grease, glue or other construction contaminants and sand wood as
required. Routed areas on MDF board should be sanded with a fine grade of sand paper,
a minimum of 400 grit. UV filled MDF board must be sanded before application of
Clawlock Primer / Undercoater to assure good intercoat adhesion.

This is why I called them. They mention 400g for edges, but don't mention anything specific for the faces, so I was unclear on if the recommendations for "wood" applied to the faces of MDF. They guy in tech support looked it up and told me 320g.

In any case, I'm going to do some tests with various levels of surface prep and see what kind of results I get.

11/18/15       #14: Sanding MDF for paint ...
Paul Snyder  Member

Website: finishing.tips

I usually use 150 for pretty much everything, but like Adam I also prefer 220 on MDF to avoid making the surface too fuzzy. I also use the same grit on the edges so it won't soak up all the primer. This single sanding step works for me and the adhesion is good - no problems.

The picture shows an example where I sanded the right half of the panel edge with 220 and the primer didn't soak in like it did on the left side (sanded to a higher grit).


View higher quality, full size image (681 X 511)

11/18/15       #15: Sanding MDF for paint ...
JeffD

So what your saying is the "tech" you spoke to contradicted ML's printed recommendations? I'm not sure I'd want to talk with that guy again!

All I can tell you is I've got a lot of mdf panels out there and not a single one has ever been sanded past 150, and most just to 120 grit. I've never had a problem….but that's just my experience. Oh and edges/profiles are completely different, then you do have to up the anti in terms of grit or it's a real pain to get a smooth finish.

good luck,
JeffD

11/18/15       #16: Sanding MDF for paint ...
Adam West  Member

Website: http://www.surfprepsanding.com

I am one of those sand paper suppliers that must only want to get you to buy more sandpaper according to Kevin.

My reputation in the industry is one of saving customers money.

Sanding to 120 or 150 grit can work. It just uses more material to fill the surface. You can sand with 80 grit if it tickles your fancy.

MDF likes to be polished a bit to help avoid too much material soaking in. The more you fluff up the surface the more the material soaks in.

I work with ML Campbell, Chemcraft, Akso Nobel, Sherwin Williams, Gemini, and several other coatings companies. They all have their various ways of trying to fill the grain on MDF.

Too much solids and the material won't flow out and you will have bad orange peel. Too thin and it just doesn't fill.

The best MDF flat surface I have seen so far was sanded to 220, sprayed with a light coat of thin primer to seal the surface, sanded to 280 grit, then primed again with a primer with good flow and the surface will look much flatter and cleaner. 280 again before paint.

The best profiles I have seen were sanded to 320 first. Then sanded with a 150 grit double sided sponge after the first and second coats. The equivalent of 320 grit again.

I hate to watch people load on huge amounts of primer, leaving a nasty lumpy mess, and then sand most of it off in an attempt to get the surface flat again. I watch customer after customer waste 80% or more of their primer by sending up the dust collector and they never get how insanly silly that is......

11/19/15       #17: Sanding MDF for paint ...
Louis Brandt

I spoke with ML Campbell again this morning, and 320g. is the recommendation. See the attached MDF Guide. After seeing all of your posts, I started to wonder whether what the tech I spoke with was referring to the grit to use when sanding between coats when he told me 320g.

Click the link below to download the file included with this post.

MDF_guide.PDF

11/19/15       #18: Sanding MDF for paint ...
Rick Mosher  Member

Website: profinisher.blogspot.com/

On the face of MDF you are sanding between coats of finish as there is a UV coating already on the sheet.

11/19/15       #19: Sanding MDF for paint ...
Louis Brandt

We are sanding between coats of primer and finish, 320g I believe. My question was how much the face of the MDF needs to be sanded before the first coat of primer is applied. My finisher and ML Campbell both say 320g. I'm not sure if the MDF we use is UV filled or not.

11/19/15       #20: Sanding MDF for paint ...
Paul Snyder  Member

Website: finishing.tips

Louis - the data sheet they sent you does say to sand the face of raw MDF with 320 or to use 180 if it's pre-primed from the factory (UV filled). You would know if you're using pre-primed/sealed MDF. The sheet goes on to say that you should pre-seal the MDF with a coat of highly thinned Magnalac if it's a lower density product that gets very fuzzy when sanded. That's an extra step and I don’t know anybody that does it. Let me point out that the data sheet does not say to work your way through all the grits up to 320. It says to use 320 (only). That's a very important distinction that will save a LOT of time and material immediately.

It may be that the technique outlined in the data sheet is the best approach. It's also possible there's a better way. In this thread some experienced finishers offered their advice and they use different approaches to achieve the same results. That tells me there’s more than one to get the job done. The one thing most everyone seems to agree on is that 320 is too fine.

Chances are some of the approaches are more cost-effective than others in terms of efficiency and/or cost of materials. Though sometimes a savings in material is offset by an expense in labor (and vice versa). It's a balancing act.

At this point I’d recommend you do some testing to find the approach that is most cost effective and produces the standard of quality you need to make the customer happy. There are some variables that can affect what will work best for you including the grade of MDF you use, the techniques used by the people doing the sanding, the type of the sandpaper, the techniques the spray operator uses, etc..

Start by sanding half of a 4x8 panel with 150 and the other half with 220. Do not work your way through all the grits - use these single grits ONLY. Then sand the edges on one half with 220 and use 320 on the other half. Perform the work quick and easy – do not take extra time to make it better than usual.

Now spray the whole panel with a coat of primer thinned about 20% (or more if that’s your standard procedure). Sand the panel with 220 or 320 to smooth and spray another coat of primer (thinned per your preference). Sand with 320 to smooth and topcoat.

Let the panel dry for 3 days in a warm, well ventilated space and then evaluate the visual difference between the 2 halves. Do an adhesion test on each half. Choose the side that looks the best, adheres well, and takes the least amount of work/time. Start using that process on a regular basis but keep an eye on the quality and labor hours. Do another adhesion test in couple weeks just to follow up. As a matter of routine, make sure the sanding crew isn’t using worn out sandpaper.

Find out if your company always orders the same quality MDF - some are denser than others and are easier to paint (less coats of primer). The standardized process you come up with will have to adapt if your supplier sends you a different grade of MDF one day, so you should be familiar with what you’re getting and how it behaves from a machining and finishing perspective.

Lastly, if you get a chance, report back on the results of your testing and the process that works best for you.

11/20/15       #21: Sanding MDF for paint ...
Kevin

i like the above post. see what works for you.. .

and on a side note, i would be weary of any process that produces finishes that cannot hold up to blue (low-tack) tape.. if the paint is pulling off by using blue paint you have an adhesion issue, and the process must be reviewed.

11/20/15       #22: Sanding MDF for paint ...
Louis Brandt

Guys, thanks for your help, this has been great. I'm going to take this to the lab and do some serious testing. I'll post my results. Thanks again.

11/22/15       #23: Sanding MDF for paint ...
scott

I use Becker Aroma and my supplier for years has said don't sand anything past 180.
It doesn't matter what grit you sand with, you are going to get grain lift, that is what liquid on wood does. Thats when you give it a good sanding with a fine grit, I use 320 for clear and coarser for solid color.
In your case the quality of finish sounds like all your concerned about so as others have said, just finish a couple panels that have been sanded to 150 and 320, Complete your schedule for finishing and compare them. You then have to decide if the extra sanding is important for your finished product or is it an extra expense? good luck.

11/24/15       #24: Sanding MDF for paint ...
Denny J

Claw lock would certainly require less prep sanding than Aqualente. Personally I have shot tons of both and have found that 150 grit works for us and gives great results. I find that a thinner first coat makes a bigger difference than using that many sanding levels.JMHO

12/4/15       #25: Sanding MDF for paint ...
Adam

We've always done 150 grit for wood.

If we are trying to get a good quality finish on mdf like raised panels. Then we sand the exposed edge to 240 grit. Spot prime with BIN or Clawlock. Sand with 320 then spray the whole panel.

There should be no adhesion issues on exposed edges of mdf. Its like a sponge. The finish is literally absorbed.

12/4/15       #26: Sanding MDF for paint ...
Adam

We don't sand the original faces ever. The material is so porous the idea of roughing it up to promote adhesion is not relevant.

12/4/15       #27: Sanding MDF for paint ...
Louis Brandt

My test samples are in the finishing room now, I should know soon what works best.

12/31/15       #28: Sanding MDF for paint ...
Steve G.

It is time to move to the 21st century,as a finisher for the ultra high end furn.industry for over thirty years the best method to finish mdf. is to sand the edges to 320 and the surface to 320 as well,and seal the MDF. first , with either a Catalyzed vinyl sealer. S.W makes the best, reduced to penetrate into the MDF.or use Ilva poly sealer.
Sand to 320 then prime. When you seal first there will be no micro voids bet the primer and the MDF.therefore no more shrinkage and your edges will look totally filled forever.And by the way the primer really holds on to the sealed MDF.NO masking issues.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!