GF Enduro CV Problems on Oak

4/2/16       
Dave Member

Website: http://davescustomservices.com

I am in the process of re-finishing a Red Oak dining table top for a customer and I am getting "pin holes" in the surface of the open grain areas on the final top coats. I have done many of these with no issues and fantastic results. This one is not going well at all. Here is what I have done so far.

1st Attempt: Took the table apart, ran the panels through the sander, finish sanded to 180, raised the grain with a wet sponge, let dry, applied 2 coats of rtm stain, applied 1 coat of enduro sanding sealer, sanded, applied 3 coats of satin enduro CV. The first coat looked weird, looked like little craters in the surface while still wet. As it dried the craters closed up into tiny little pin holes. Called GF and he said solvent pop, I was not waiting long enough between coats, give it 2 hours instead of one, ok, did a final coat the next morning, looks like sh**. Called GF again, he said give a few days it will shrink down. ok. waiting, waiting, looks the same, can't take it any more. Sanded it all off and try again.

2nd attempt: Sanded all back to bare wood. applied 1 coat stain, lightly sanded raised grain, apply 2nd coat of stain, lightly sand, (with advice from GF) apply one coat of GF Armrseal, sand, apply one coat of sanding sealer, sand, apply cv, let dry 3 hours between coats, better but still looks like sh** with tiny little holes in it.

Tried again on a leaf except with just enduro clear poly, better, but still little holes in it. The little holes are only noticeable in the light, but you can feel them, you can feel the grain too real good. It is like the wood is the problem. I did a Walnut top earlier in the week, same steps as above, fantastic results. Did a veneered oak top a couple weeks ago and looks great. At this point I am thinking of sanding it all back down and using a solvent base finish. I always have trouble with water base finishes on oak. Maple, Cherry, Walnut turn out great.

And yes the cv and catalyst was mixed with a power mixer for 5 minutes and sweated in for 30 minutes.


View higher quality, full size image (2560 X 1440)


View higher quality, full size image (2560 X 1440)


View higher quality, full size image (2560 X 1440)

4/2/16       #2: GF Enduro CV Problems on Oak ...
rich c.

Looks like air bubbles from the course grain. I'd suggest thinner coats of finish. Do they make a retarder for that finish to slow drying?

4/2/16       #3: GF Enduro CV Problems on Oak ...
Leo G Member

Can you put a retarder in the finish. I'm a solvent guy, so I don't know.

If you can use the retarder and spray very thin coats. Oak is problematic and pinholes go with the wood.

Light coats will help with the pinholes. They are usually caused by the deep grain and the inability of the finish to bridge the grain. When you put a thick coating on it, it can't bridge and it'll form pockets that the finish can't bridge.

4/4/16       #4: GF Enduro CV Problems on Oak ...
RobertJ

You could try a barrier coat of 'De-waxed' shellac and see how that goes.....it may change the color depending upon the grade and color the shellac flakes. Got to make samples. If you don't have flakes, try Zinsser 'Sealcoat' which costs as little as 13.00 per quart. Worth a try.

4/4/16       #5: GF Enduro CV Problems on Oak ...
Bart

I also use GF but not their CV yet. I don't do Red Oak but I think it goes with the territory with WB. Mahagony can bridge like that with multiple coats it's just the nature of WB on those species.
They only recommend 5% thinning of CV but you can add their retarder/extender or just do lighter coats. Also it will tighten up somewhat. I've gone back on jobs and the finish looked way tighter than when it left the shop.

Also I gotta say your schedule looks like over kill to me. I'll never understand the raising the grain thing. I've never done it in over 15yrs of finishing for $$$. You're doing multiple sands anyway. I don't get the Armrseal either it's an oil based product? Why add complexity to the process? The CV or Poly would be fine for a table top. I've done multiple desks, countertops and tabletops and have used the pre-cat in the past and now the poly. If it were my project I'd stick to the poly and call it a day. You can thin it how you like and no catalizing. Unless you're putting glass over it every finish scratches including glass.

4/4/16       #6: GF Enduro CV Problems on Oak ...
Dave Member

Thank you for the input.

Looks like a grain filler is needed. I have found that there is a grain filler called Timbermate, needs to go on before staining. And a product called Crystalac, a water based clear filler that can go on after the finish, then just top coat it. I am going to leave it the way it is and use the Crystalac. I will post pics of it if it works and let you know. I also ordered the timbermate I will try on the next oak top and see which I like better. I am new to grain fillers so this will be interesting to see how it turns out.

4/9/16       #7: GF Enduro CV Problems on Oak ...
Sean Jackson Member

I wouldn't have thought a grain filler is the remedy here. I have this issue when shooting CV over oak sometimes. I just come at it with a few mist coats to start with, then just carry on with thinner finish than usual, just going slower and thinner basically. If it's just the odd time it occurs that's workable, if I were seeing this all day long i'd be looking at a clear dewaxed shellac sealer initally or similar.

4/12/16       #8: GF Enduro CV Problems on Oak ...
Nick

Not GF but when it comes to leveling and a close to the wood wb finish Targets pre-cat 8000 CV does an amazing job.

4/13/16       #9: GF Enduro CV Problems on Oak ...
Dave

Thanks for all the info folks. After re sanding 2 times, and using a grain filler, still saw a few pin holes coming through. 5 coats of oil based poly urethane on top of a grain filler and still had a few pin holes. There must be something in the wood? The wood will not close up. It looks pretty good now. I did other pieces of oak from my lumber and had no problems as I went. Just on this funky wood. Another woodworker friend suggested that the wood may have been dead when harvested, after sanding the wood did look very white like sap wood?? Would have been better off to re make the top from new wood I think.

4/13/16       #10: GF Enduro CV Problems on Oak ...
Robert Member

Try block sanding a scrap piece with 150. The larger the pad the better. Then complete the finishing procedure.

5/21/16       #11: GF Enduro CV Problems on Oak ...
Steve G.

in my 30 plus years as a finisher ,when water born was going to be the next big thing all my reps,gave me gallons as samples to try and I DID,THE TRUTH IS THAT THEY REALLY DID NOT IMPROVE THEM TOO MUCH.......From your pic, I see that your application is too heavy on your topcoat,water has a high amount of surface tension therefore the product dose `nt bridge gaps very well unless you flood it on and hope for the best and still looks like crap.Oak and waterborn just suck together.Here is your solution first a coat of vinyl sealer Sherwin Williams is the best,when fully cured give One coat at a time of your waterborn topcoat mixed with a small amount of BUTYL CELLOSOLVE will help the product flow out.Let each coat cure before application of next and if you do a more thorough sanding between coats the finish wont be as lumpy and you will have a good looking open pore finish .flat smooth and nice and crisp grain definition....Let me know how you make out.

6/16/21       #12: GF Enduro CV Problems on Oak ...
Randi Gentile Member

I was looking for info on the web about holes in oak. I bought a table and right after I got it, this stuff started coming out. It is caused by an insect call a false powder post beetle. They love oak. That's what caused the damage to your table. Not sure what to do about it, but good luck. Just had to tell you.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production

    Become a Sponsor today!