Problems with MagnaMax H2O

9/18/19       
Chuck Member

I decided to give MagnaMax H2O a try, and I am having some trouble with bubbles in the finish on the table tops. A lot of bubbles. It’s pretty bad. Not having any on vertical surfaces.
My setup:
60 gal puma 5 HP compressor
Cat-x gun with 1.3 tip and pps cup
Using recommended 35 psi pressure at gun. I tried lowering the pressure to 29 and it did not help.

I called ca technologies and he suggested moving up to the 1.7 tip??? I just don’t think that’s right given how thin this stuff is.

Has anyone had success spraying this stuff? If so, can you provide me any help or guidance?

Thank you!

9/18/19       #2: Problems with MagnaMax H2O ...
rich c.

What film thickness? My guess is you are laying it on too thick.

9/18/19       #3: Problems with MagnaMax H2O ...
Leo G Member

That's my guess too.

9/19/19       #4: Problems with MagnaMax H2O ...
JaySun

Thick coats will cause issues with that. With water borne best to use a little thinner coats even though this is a urethane type coating still best to lean towards thinner coats.

9/19/19       #5: Problems with MagnaMax H2O ...
JoeW Member

Been using it consistently for a while now.

Definitely thin coats as all have said.

Also, do not rush drying. Limit air movement over it until it crust over. Bubbles get trapped when dries too fast.

I use fans to move air when I use the Agualente. Stopping that with the Magnamax H2O made a big difference.

9/19/19       #6: Problems with MagnaMax H2O ...
Mark B Member

Ive been spraying it straight with a 1.2 I cant imagine going to a 1.7

My biggest complaint is the stuff smells like rotten milk or something.

9/19/19       #7: Problems with MagnaMax H2O ...
DannyB Member

The reason they are likely suggesting a 1.7 tip is, i guess strangely, the reason you are seeing the other advice.

As others say, you need thin coats and want to not get air trapped in it.

While the 1.7 will not help with thickness (you'd obviously have to be more careful), it will atomize it less and entrap less air into it.

Put another way: the 1.3 tip may be breaking it up into small enough particles that you are getting a bunch of air trapped in the coat.

The 1.7 will definitely help with that if it's the issue.

But you do have to be more careful about coating thickness, turn down the fluid, etc.

At the same time, it is likely you can fix it with technique/lowering air as well, spraying thinner coats, and staying with a 1.3 tip.

9/19/19       #8: Problems with MagnaMax H2O ...
Mark B Member

I just ordered a 1.7 for the heck of it. I cant imagine being able to control WB with such a large tip. Ive never had a tip that large for clears. It would seem a precarious situation and nearly impossible on verticals but fun to try. I always assume that most just think WB clears are thick and need a bigger tip by default. That hasnt been the case across the board for me.

I thought the film build was likely the issue given the problem only showing up on horizontal surfaces though no mention of the substrate.

9/19/19       #9: Problems with MagnaMax H2O ...
DannyB Member

Yeah, magnamax h20 is definitely very thin (It's 18 seconds ford #4).

The only reason i'd consider giving it a try is that historically, CAT and ML campbell had a very close relationship.

(I dunno if this is still true after CAT was acquired by wagner).

CAT used to publish and update guides with good settings for ML Campbell products, and it used to be very easy to get MLC folks to help as well.

I haven't seen the guide updated in a while, however, so not sure if they still have the same close relationship they used to.

9/23/19       #10: Problems with MagnaMax H2O ...
Jonathan Mahnken

could also be a problem with low humidity. do spray thin as you can and still get nice flow.

9/23/19       #11: Problems with MagnaMax H2O ...
Jim Member

I had that problem with it when spraying red oak. The first two coats look like hell, but the third coat just flattened out.


Post a Response
  • Notify me of responses to this thread
  • Subscribe to email updates on this Forum
  • To receive email notification of additions to this forum thread,
    enter your name and email address, and then click the
    "Keep Me Posted" button below.

    Please Note: If you have posted a message or response,
    do not submit this request ... you are already signed up
    to receive notification!

    Your Name:
    E-Mail Address:
    Enter the correct numbers into the field below:
     

    Date of your Birth:



    Return to top of page

    Buy & Sell Exchanges | Forums | Galleries | Site Map

    FORUM GUIDELINES: Please review the guidelines below before posting at WOODWEB's Interactive Message Boards (return to top)

  • WOODWEB is a professional industrial woodworking site. Hobbyist and homeowner woodworking questions are inappropriate.
  • Messages should be kept reasonably short and on topic, relating to the focus of the forum. Responses should relate to the original question.
  • A valid email return address must be included with each message.
  • Advertising is inappropriate. The only exceptions are the Classified Ads Exchange, Machinery Exchange, Lumber Exchange, and Job Opportunities and Services Exchange. When posting listings in these areas, review the posting instructions carefully.
  • Subject lines may be edited for length and clarity.
  • "Cross posting" is not permitted. Choose the best forum for your question, and post your question at one forum only.
  • Messages requesting private responses will be removed - Forums are designed to provide information and assistance for all of our visitors. Private response requests are appropriate at WOODWEB's Exchanges and Job Opportunities and Services.
  • Messages that accuse businesses or individuals of alleged negative actions or behavior are inappropriate since WOODWEB is unable to verify or substantiate the claims.
  • Posts with the intent of soliciting answers to surveys are not appropriate. Contact WOODWEB for more information on initiating a survey.
  • Excessive forum participation by an individual upsets the balance of a healthy forum atmosphere. Individuals who excessively post responses containing marginal content will be considered repeat forum abusers.
  • Responses that initiate or support inappropriate and off-topic discussion of general politics detract from the professional woodworking focus of WOODWEB, and will be removed.
  • Participants are encouraged to use their real name when posting. Intentionally using another persons name is prohibited, and posts of this nature will be removed at WOODWEB's discretion.
  • Comments, questions, or criticisms regarding Forum policies should be directed to WOODWEB's Systems Administrator
    (return to top).

    Carefully review your message before clicking on the "Send Message" button - you will not be able to revise the message once it has been sent.

    You will be notified of responses to the message(s) you posted via email. Be sure to enter your email address correctly.

    WOODWEB's forums are a highly regarded resource for professional woodworkers. Messages and responses that are crafted in a professional and civil manner strengthen this resource. Messages that do not reflect a professional tone reduce the value of our forums.

    Messages are inappropriate when their content: is deemed libelous in nature or is based on rumor, fails to meet basic standards of decorum, contains blatant advertising or inappropriate emphasis on self promotion (return to top).

    Libel:   Posts which defame an individual or organization, or employ a tone which can be viewed as malicious in nature. Words, pictures, or cartoons which expose a person or organization to public hatred, shame, disgrace, or ridicule, or induce an ill opinion of a person or organization, are libelous.

    Improper Decorum:   Posts which are profane, inciting, disrespectful or uncivil in tone, or maliciously worded. This also includes the venting of unsubstantiated opinions. Such messages do little to illuminate a given topic, and often have the opposite effect. Constructive criticism is acceptable (return to top).

    Advertising:   The purpose of WOODWEB Forums is to provide answers, not an advertising venue. Companies participating in a Forum discussion should provide specific answers to posted questions. WOODWEB suggests that businesses include an appropriately crafted signature in order to identify their company. A well meaning post that seems to be on-topic but contains a product reference may do your business more harm than good in the Forum environment. Forum users may perceive your references to specific products as unsolicited advertising (spam) and consciously avoid your web site or services. A well-crafted signature is an appropriate way to advertise your services that will not offend potential customers. Signatures should be limited to 4-6 lines, and may contain information that identifies the type of business you're in, your URL and email address (return to top).

    Repeated Forum Abuse: Forum participants who repeatedly fail to follow WOODWEB's Forum Guidelines may encounter difficulty when attempting to post messages.

    There are often situations when the original message asks for opinions: "What is the best widget for my type of shop?". To a certain extent, the person posting the message is responsible for including specific questions within the message. An open ended question (like the one above) invites responses that may read as sales pitches. WOODWEB suggests that companies responding to such a question provide detailed and substantive replies rather than responses that read as a one-sided product promotion. It has been WOODWEB's experience that substantive responses are held in higher regard by our readers (return to top).

    The staff of WOODWEB assume no responsibility for the accuracy, content, or outcome of any posting transmitted at WOODWEB's Message Boards. Participants should undertake the use of machinery, materials and methods discussed at WOODWEB's Message Boards after considerate evaluation, and at their own risk. WOODWEB reserves the right to delete any messages it deems inappropriate. (return to top)


  • Forum Posting Help
    Your Name The name you enter in this field will be the name that appears with your post or response (return to form).
    Your Website Personal or business website links must point to the author's website. Inappropriate links will be removed without notice, and at WOODWEB's sole discretion. WOODWEB reserves the right to delete any messages with links it deems inappropriate. (return to form)
    E-Mail Address Your e-mail address will not be publicly viewable. Forum participants will be able to contact you using a contact link (included with your post) that is substituted for your actual address. You must include a valid email address in this field. (return to form)
    Subject Subject may be edited for length and clarity. Subject lines should provide an indication of the content of your post. (return to form)
    Thread Related Link and Image Guidelines Thread Related Links posted at WOODWEB's Forums and Exchanges should point to locations that provide supporting information for the topic being discussed in the current message thread. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related Link that directs visitors to an area with inappropriate content will be removed. WOODWEB reserves the right to delete any messages with links or images it deems inappropriate. (return to form)
    Thread Related File Uploads Thread Related Files posted at WOODWEB's Forums and Exchanges should provide supporting information for the topic being discussed in the current message thread. Video Files: acceptable video formats are: .MOV .AVI .WMV .MPEG .MPG .MP4 (Image Upload Tips)   If you encounter any difficulty when uploading video files, E-mail WOODWEB for assistance. The purpose of WOODWEB Forums is to provide answers, not to serve as an advertising venue. A Thread Related File that contains inappropriate content will be removed, and uploaded files that are not directly related to the message thread will be removed. WOODWEB reserves the right to delete any messages with links, files, or images it deems inappropriate. (return to form)
    Sponsors
    • TotalFinishingSUPPLIES.com
      Solutions and supplies from spray tips to spray booths for all your woodworking needs
    • Unique Machine & Tool
      Industrial Machinery for Door and Drawer Production
    • EX-FACTORY INC.
      Offering New & Used Woodworking Machinery including Auctions & Liquidations
    • Simantech
      New & Used Machinery, Supplies, Tooling, Parts, and Abrasive Products

    Become a Sponsor today!